Treatment and resource recovery methods of waste lithium-ion batteries
Through the overall drying method of drilling and infrared evaporation, the safety risks and low efficiency problems in waste lithium-ion battery processing and resource recycling are solved, and efficient and low-energy-consuming electrolyte removal and material separation are achieved, and product purity and Recovery rate.
Patent Information
- Application Number
- CN202411088540.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing waste lithium-ion battery treatment and resource recycling methods have problems such as high safety risks, low processing efficiency, high energy consumption, high cost, low separation efficiency and low product purity, making it difficult to achieve harmless treatment and resource recycling.
The integrated drying method of drilling and infrared evaporation is adopted to discharge waste lithium-ion batteries and form exhaust holes on one side. The electrolyte is removed at 120℃ to 140℃ by using infrared radiation to avoid the risk of electrolyte leakage and explosion. And separate separation of the positive electrode, negative electrode and the separator is achieved through steps such as reverse winding and crushing.
It improves processing safety, efficiency and purity, reduces energy consumption and cost, realizes high recovery rate and high-quality separation of positive and negative electrode material powders, and ensures harmless treatment and resource recycling of waste lithium-ion batteries.
Smart Images

Figure CN118659056B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waste lithium-ion battery treatment and resource recovery, and relates to a waste lithium-ion battery treatment and resource recovery method. Background Art
[0002] As the function and efficiency of lithium-ion batteries deteriorate and even fail, a large number of waste lithium-ion batteries are generated. At the same time, waste lithium-ion batteries contain a large number of valuable heavy metals, such as nickel, cobalt, manganese, copper, aluminum, etc., and also contain a large number of organic substances, such as fluorine-containing organic substances, organic solvents such as esters, ethers, sulfones, nitriles and nitro compounds, as well as organic additives such as SEI film-forming additives, positive electrode protection additives, lithium salt stabilizers, overcharge and overdischarge protection agents and flame retardant additives, as well as binders such as PVDF and PTEE; secondly, since waste lithium-ion batteries also contain a large number of flammable and explosive components, if they are improperly operated during the disassembly and resource recovery process, they may cause fire and explosion, heavy metal pollution, organic waste gas emissions and other problems, and also endanger the life and property of operators. Therefore, how to safely and effectively treat waste lithium-ion batteries and realize the resource utilization of waste lithium-ion batteries is of great significance.
[0003] The existing methods for processing and recycling waste lithium-ion batteries mainly include the following two methods:
[0004] like Figure 1As shown, the first recycling process is the traditional process A, which includes the following steps: discharging the battery; crushing the discharged battery as a whole to form crushed materials; placing the crushed materials in a rotary kiln for drying and sorting, separating the positive electrode, negative electrode, and diaphragm from the current collector, and then collecting black powder (positive and negative electrode powder), copper particles, and aluminum particles through operations such as crushing, screening, grinding, and sorting; at the same time, the tail gas collected during the crushing and rotary kiln drying process is condensed and the condensed components are recovered, and can also be transferred to the combustion chamber to be burned together with the diaphragm obtained by subsequent sorting, and the combustion tail gas is discharged after subsequent treatment to meet the standards. The main defects of this process method are: (1) Directly crushing the battery is prone to explosion and deflagration due to the presence of electrolyte, which has a high safety risk. At the same time, it is also easy to cause electrolyte splashing, resulting in a harsh working environment, high requirements for equipment, and strict requirements for process conditions. (2) The processing process is complicated, the processing efficiency is low, and it is difficult to achieve batch processing. (3) The use of a rotary kiln for drying is a dynamic drying method, which is prone to flash explosions caused by blockage due to powder gas stickiness, and is likely to bring more powder into the exhaust gas, resulting in a significant increase in the amount of powder loss. It also makes the composition of the exhaust gas complex, making subsequent treatment more difficult and the risk of secondary pollution high. (4) The separation of the various components is difficult, the separation efficiency is low, the recovery rate is low, and there are many impurities. (5) After high-temperature treatment in a rotary kiln, the pole piece becomes brittle, and the diaphragm and binder melt, coke or carbonize, causing the positive and negative electrode materials to stick together and be difficult to separate, and causing the pole piece material powder to enter the positive electrode material, making it difficult to quickly separate the various components, with low separation efficiency and low recovery volume. In addition, the impurity content in the resulting black powder is high, which is not conducive to subsequent resource utilization.
[0005] In view of the above defects in traditional process A, researchers have proposed improvement plans, such as Figure 2As shown, the second recycling process is the traditional process B, which includes the following steps: discharging the battery; precisely disassembling the discharged battery, removing the battery shell, and obtaining the battery cell; crushing the battery cell to form crushed materials; placing the crushed materials in an infrared low-temperature furnace for drying, grinding and sorting, separating the positive electrode, negative electrode, and diaphragm from the current collector, and then collecting black powder (positive and negative electrode powder), copper particles and aluminum particles through operations such as crushing, screening, grinding, and sorting. Although the impurity content in the black powder can be reduced by removing the shell in advance in the traditional process B, this also makes the recycling process more complicated and the recycling efficiency lower; at the same time, in the process of disassembling the battery cell, it is also prone to explosion, deflagration and other risks, and it is easy to cause electrolyte leakage, which brings higher safety risks to operators and higher requirements for equipment and process conditions, and ultimately leads to higher recycling costs. In addition, when using an infrared low-temperature drying furnace to dry the battery cell crushed materials, the crushed materials are in a "stacked state", resulting in low heat exchange efficiency, and therefore require more energy and higher temperatures to remove the electrolyte. There are still shortcomings such as poor electrolyte removal effect, high energy consumption, and long drying time. At the same time, drying under high temperature conditions can easily lead to embrittlement of the pole pieces, melting, coking or carbonization of the diaphragm and binder, thereby causing the positive and negative electrode materials to stick together and be difficult to separate, and causing the pole piece material powder to enter the positive electrode material, resulting in difficulty in rapid separation of the components, low recovery rate, and high impurity content in the resulting black powder, which is not conducive to subsequent resource utilization.
[0006] Therefore, obtaining a method for treating and recycling waste lithium-ion batteries with high safety factor, high processing efficiency, low energy consumption, low cost, high product recovery rate, high product purity and good economic benefits is of great significance for realizing batch processing of waste lithium-ion batteries and improving the social and economic benefits of waste lithium-ion batteries.
[0007] In addition, the existing methods for removing electrolyte from waste lithium-ion batteries still have defects or deficiencies such as low processing efficiency, poor removal effect, large loss of positive and negative active materials, high safety risk, high energy consumption, high cost, and easy secondary pollution, which also makes it difficult for the existing waste lithium-ion battery treatment process to overcome the defects such as low safety factor, low processing efficiency, high energy consumption, high cost, difficulty in separating each component separately, low product recovery rate, low product purity, and poor economic benefits, which ultimately makes it difficult to achieve harmless treatment and resource recycling of waste lithium-ion batteries. So far, there has been no report on "using the overall drying method combined with punching and infrared evaporation to remove electrolyte from waste lithium-ion batteries". Therefore, obtaining a method for removing electrolyte from waste lithium-ion batteries with high processing efficiency, good removal effect, small loss of positive and negative active materials, high safety factor, low energy consumption, and green environmental protection is of great significance for promoting harmless treatment and resource recycling of waste lithium-ion batteries. Summary of the invention
[0008] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for processing and recycling waste lithium-ion batteries with high safety factor, high processing efficiency, low energy consumption, low cost, high product recovery rate, high product purity and good economic benefits.
[0009] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0010] A method for processing and recycling waste lithium-ion batteries comprises the following steps:
[0011] S1. Discharging the waste lithium-ion batteries;
[0012] S2, punching holes in the outer shell of the waste lithium-ion battery after the discharge treatment to form an exhaust hole on one side of the waste lithium-ion battery; the diameter of the exhaust hole is 4 mm to 6 mm;
[0013] S3, with the exhaust hole facing upward, performing infrared evaporation on the waste lithium-ion battery to remove the electrolyte in the waste lithium-ion battery; the infrared evaporation is performed at a temperature of 120° C. to 140° C.;
[0014] S4, dismantling the waste lithium-ion batteries after infrared evaporation and taking out the battery cells;
[0015] S5, reversely winding the battery cell to obtain a positive electrode, a negative electrode and a separator;
[0016] S6. The positive electrode and the negative electrode are crushed respectively to obtain positive electrode material powder, negative electrode material powder, aluminum powder and copper powder, thereby completing the treatment and resource recovery of waste lithium-ion batteries.
[0017] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved in that the exhaust hole is located on the surface close to one end of the electrode of the waste lithium-ion battery; the distance between the exhaust hole and the edge close to one end of the electrode of the waste lithium-ion battery is ≤10mm.
[0018] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved in that the number of the exhaust holes is 3 to 9, which are distributed in a row on the surface near one end of the electrode of the waste lithium-ion battery, and the distance between every two exhaust holes is 10 mm to 30 mm.
[0019] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved. In step S2, the shell of the waste lithium-ion battery after discharge treatment is punched by acupuncture; the depth of the exhaust hole is the same as the thickness of the shell.
[0020] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved. In step S3, infrared radiation is used to perform infrared evaporation on the waste lithium-ion batteries, so that the electrolyte in the waste lithium-ion batteries is vaporized and discharged from the exhaust hole; the wavelength of the infrared radiation is 5μm to 25μm; and the time of the infrared evaporation is 75min to 90min.
[0021] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved by using an infrared heating plate as an infrared radiation source to perform infrared evaporation on the waste lithium-ion batteries; the infrared heating plate is located above the waste lithium-ion batteries, and / or the infrared heating plate is located below the waste lithium-ion batteries, and / or the infrared heating plate is located on the side of the waste lithium-ion batteries; the infrared heating plate includes an insulation layer, an infrared heating layer and a heat-conducting layer stacked in sequence from bottom to top; the infrared heating layer is a graphene heating layer, and the graphene heating layer is bonded to the heat-conducting layer; the heat-conducting layer is a microcrystalline glass plate.
[0022] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved, in which in step S1, the waste lithium-ion batteries include lithium iron phosphate batteries and / or ternary lithium batteries.
[0023] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved, and step S3 also includes the following processing: collecting the exhaust gas generated during the infrared evaporation process; using plasma combustion technology to burn the exhaust gas; and the exhaust gas generated during the combustion process is discharged after dust removal.
[0024] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved. In step S5, the subsequent processing of the diaphragm includes the following steps: burning the diaphragm; and exhausting the waste gas generated during the combustion process after dust removal.
[0025] The above-mentioned method for processing and recycling waste lithium-ion batteries is further improved. In step S6, before crushing the positive electrode and the negative electrode, the following processing is also included: using an infrared drying furnace to dry the positive electrode and the negative electrode respectively; the drying temperature is 170°C to 210°C; the drying time is 30min to 60min.
[0026] Compared with the prior art, the advantages of the present invention are:
[0027] (1) In view of the defects of the existing waste lithium-ion battery treatment methods such as low safety factor, low treatment efficiency, high energy consumption, high cost, difficulty in separating the components separately, low product recovery rate, low product purity and poor economic benefits, the present invention creatively proposes a waste lithium-ion battery treatment and resource recovery method, which first discharges the waste lithium-ion battery to avoid short circuit and possible runaway reaction in the subsequent punching process, and further, punches the shell of the waste lithium-ion battery after the discharge treatment to form an exhaust hole on one side of the waste lithium-ion battery, and controls the aperture of the exhaust hole to be 4mm to 6mm, by only An exhaust hole is set on one side of the battery and the aperture of the exhaust hole is optimized. On the one hand, it can effectively prevent the leakage of the electrolyte. On the other hand, in the subsequent infrared evaporation process, it is also conducive to forming a pressurized pressure cavity inside the battery, which is convenient for the vaporization of the electrolyte. On this basis, the exhaust hole is facing upward and the waste lithium-ion battery is subjected to infrared evaporation. In this process, the electrolyte in the battery is heated by infrared radiation, which can quickly raise the temperature in the battery to the decomposition and volatilization temperature of the electrolyte, so that the electrolyte can be quickly vaporized in the battery to form electrolytic gas. When the gas pressure in the battery reaches a certain level, the electrolytic gas can be discharged through the exhaust hole. The electrolyte in the waste lithium-ion battery is discharged outward through the pores, thereby completing the removal of the electrolyte in the waste lithium-ion battery; at the same time, the battery is directly heated by infrared radiation, and the electrolyte can be vaporized at a lower temperature, which is beneficial to reduce the adverse effects of the heating temperature on other components in the battery, such as reducing the loss of powder, preventing the electrode sheet from becoming brittle, and preventing the diaphragm and binder from being carbonized. In particular, the pressure that can be formed in the battery by directly heating the battery with infrared radiation is less than the safety pressure of the battery, thereby ensuring that the battery will not explode during the heating process, and the safety factor is higher; more Most importantly, the overall drying method of punching combined with infrared evaporation is used to remove the electrolyte in the battery, which will not destroy the original components and structure of the battery, and is conducive to the individual separation of each component in the subsequent process. It has high separation efficiency, high recovery volume and high purity. While achieving the individual separation of each useful component, higher quality products can also be obtained. Finally, by disassembling, rewinding and crushing the waste lithium-ion batteries after infrared evaporation, high-purity and high-recovery positive electrode material powder, negative electrode material powder, aluminum powder and copper powder can be quickly separated, thereby completing the harmless treatment and resource recovery of waste lithium-ion batteries.Compared with conventional treatment methods, the treatment and resource recovery method of waste lithium-ion batteries of the present invention has the following advantages: (a) Higher safety. The overall drying method of punching combined with infrared evaporation is adopted, and the electrolyte volatilizes stably in the furnace, which is safe and controllable; after the overall drying treatment of punching combined with infrared evaporation, the electrolyte in the battery is completely removed, so in the subsequent disassembly, crushing and other stages, there will be no problems such as ignition and combustion, which is safer; infrared evaporation of the battery is a static drying method, which can overcome the flash explosion problem caused by blockage caused by sticky powder gas in the traditional dynamic drying process. (b) Higher efficiency. After the overall drying process of punching and infrared evaporation, the electrolyte in the battery is completely removed. Therefore, after removing the tabs and aluminum shell, the positive electrode, negative electrode and diaphragm in the battery cell can be separated separately by simple reverse winding, so that only the independent positive and negative electrode materials need to be processed later, which greatly improves the crushing efficiency; the deep processing link after the positive and negative electrodes are separated and crushed is highly targeted and efficient, which can also improve the recycling efficiency; the reverse winding, crushing and other links are simpler, the overall process flow is more optimized, and the processing efficiency is higher. (c) More energy-saving. The overall drying method of punching and infrared evaporation is used. Drying in a static environment, the drying atmosphere is more uniform, and energy saving is more than 20%; infrared radiation is used to heat the battery, without the need for an intermediate medium, and the transfer speed is fast, which can greatly reduce the loss in the heat energy transfer process, and the heat energy utilization rate is high; the processing flow is simpler, especially the crushing processing volume is significantly reduced, and the overall energy consumption of the production line is significantly reduced. (d) More environmentally friendly. During the entire process, waste gas is only generated in the overall drying process. The output is small and the composition is known. It can be directly discharged after plasma high-temperature combustion and dust removal. The diaphragm separated by the reverse winding process is burned separately, and the combustion effect is controllable. The waste gas generated by the combustion can also be directly discharged after dust removal. The overall static drying, reverse winding separation, and separate crushing are optimized to greatly reduce the amount of dust in the whole process. (e) Lower cost. The overall drying method is adopted, with high heat exchange efficiency, low overall energy consumption, and significantly reduced production costs. The positive and negative electrodes are treated independently, with low requirements for equipment and operators, which is conducive to reducing production costs. At the same time, the materials obtained after independent treatment have higher purity, higher recovery rate, and higher social and economic benefits. Therefore, the method for processing and recycling waste lithium-ion batteries of the present invention has the advantages of high safety factor, high processing efficiency, low energy consumption, low cost, high product recovery rate, high product purity, good economic benefits, etc., can realize batch processing of waste lithium-ion batteries, and can also recover a large amount of high-value positive and negative electrode materials from waste lithium-ion batteries, with high use value and good application prospects.
[0028] (2) In the present invention, by optimizing the diameter of the exhaust hole to 4 mm to 6 mm, it is more conducive to the rapid and thorough removal of the electrolyte while effectively avoiding the leakage of the electrolyte, and the processing efficiency is higher and the removal effect is better. This is because when the diameter of the exhaust hole is small, the discharge rate of the electrolytic gas is low, and it is difficult to discharge it quickly from the battery, resulting in poor electrolyte removal effect. When the diameter of the exhaust hole is large, the pressure in the battery is small, which is not conducive to the rapid discharge of the electrolytic gas from the battery. In particular, when the diameter of the exhaust hole is too large, it is also easy to cause electrolyte leakage.
[0029] (3) In the present invention, the opening position of the exhaust hole is optimized, specifically, the exhaust hole is located on the surface close to one end of the electrode of the waste lithium-ion battery, and the distance between the exhaust hole and the edge close to one end of the electrode of the waste lithium-ion battery is optimized to be ≤10mm. This can effectively avoid damage to the battery cell during the drilling process, not only improve the separation efficiency between the electrode and the diaphragm in the subsequent process, but also help to reduce the loss of powder (electrode active material), thereby helping to improve the resource recovery value of the battery cell.
[0030] (4) In the present invention, the number and distribution density of the exhaust holes are optimized. Specifically, the number of the exhaust holes is optimized to 3 to 9, so that the exhaust holes are distributed in a row on the surface near one end of the electrode of the waste lithium-ion battery, and the distance between every two exhaust holes is 10 mm to 30 mm, which is conducive to quickly and thoroughly removing the electrolyte from the battery.
[0031] (5) In the present invention, by optimizing the infrared evaporation temperature to 120°C to 140°C, the electrolyte in the battery can be quickly and thoroughly removed, thereby effectively avoiding adverse effects such as embrittlement of the electrode sheet and melting or carbonization of the diaphragm. This is not only beneficial for the individual separation of each useful component in the battery, but also beneficial for obtaining a product with a high recovery rate and high purity. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0033] Figure 1 The figure is a process flow chart of process A for treating waste lithium-ion batteries.
[0034] Figure 2 This is a process flow chart of process B for the existing treatment of waste lithium-ion batteries.
[0035] Figure 3 This is a process flow chart for the treatment and resource recovery of waste lithium-ion batteries in Example 1 of the present invention. DETAILED DESCRIPTION
[0036] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0037] In the following examples of the present invention, unless otherwise specified, the materials and instruments used are commercially available, the equipment used is conventional equipment, and the data obtained are the average values of more than three repeated experiments.
[0038] Example 1
[0039] A method for treating and recycling waste lithium-ion batteries, specifically treating and recycling waste ternary lithium batteries, the process flow chart of which is as follows Figure 3 As shown, the following steps are included:
[0040] S1. Discharge the waste ternary lithium battery, specifically using a constant current discharge device (conventional equipment) to provide a constant current, and discharge the waste ternary lithium battery in and out until the battery is completely discharged. Constant voltage discharge equipment (conventional equipment) can also be used to discharge the waste ternary lithium battery, but it is not limited to this. In this step, the waste ternary lithium battery is a nickel-cobalt-manganese ternary lithium battery (NCM), which is in the shape of a cuboid, 150 mm long, 120 mm high, and 80 mm thick. The method of the present invention can also be used to treat waste lithium iron phosphate batteries.
[0041] S2. Lay the used ternary lithium battery flat and feed it into the needle punching equipment. Use needle punching to punch holes in the shell of the used ternary lithium battery after discharge treatment, and form exhaust holes on one side of the used ternary lithium battery. The diameter of the exhaust holes is 6mm, and the number is 9. These exhaust holes are arranged in a row on the surface close to one end of the battery electrode, and the distance between the exhaust holes and the edge close to one end of the battery electrode is 10mm, and the distance between every two exhaust holes is 10mm. Specifically, the depth of each exhaust hole is the same as the thickness of the battery shell.
[0042] S3. With the exhaust hole facing upward, place the used ternary lithium battery flat on the infrared heating plate, make the bottom of the used ternary lithium battery fit with the infrared heating plate, use the infrared heating plate as the infrared radiation source, and use infrared radiation with a wavelength of 5μm to 25μm to perform infrared evaporation on the used ternary lithium battery. Under the action of infrared radiation, the electrolyte in the battery can be heated to 130℃ and maintained at this temperature for 75min. In this process, the electrolyte can be quickly vaporized to form electrolytic gas. When the pressure in the battery reaches a certain level, the electrolytic gas is discharged outward from the exhaust hole, thereby completing the removal of the electrolyte in the used lithium-ion battery.
[0043] In step S3, the infrared heating plate may also be arranged above the battery or on the side of the battery.
[0044] In step S3, the infrared heating plate used can be a conventional mid-infrared radiation heating plate. In this embodiment, the infrared heating plate includes a thermal insulation layer, an infrared heating layer and a thermal conductive layer stacked from bottom to top, wherein the infrared heating layer is a graphene heating layer, the graphene heating layer is bonded to the thermal conductive layer, and the thermal conductive layer is a microcrystalline glass plate.
[0045] Step S3 also includes the following processing: collecting the tail gas (electrolytic gas) generated during the infrared evaporation process, then using plasma combustion technology to burn the tail gas, collecting the waste gas generated during the combustion process, removing dust from the waste gas in and out, and discharging it after meeting the standards.
[0046] S4, dismantling the waste ternary lithium battery after infrared evaporation, specifically cutting the top cover of the battery and taking out the battery cell. In this step, the top cover and the shell obtained after dismantling can be recycled.
[0047] S5. Rewind the battery cell to obtain a positive electrode, a negative electrode and a separator.
[0048] In step S5, the subsequent treatment of the diaphragm includes the following steps: burning the diaphragm, collecting the waste gas generated during the burning process, removing dust from the waste gas, completing the harmless treatment of the tail gas, and discharging it after meeting the standards.
[0049] S6. The positive electrode is crushed to obtain positive electrode material powder and aluminum powder, and the negative electrode is crushed to obtain negative electrode material powder and copper powder, thereby completing the harmless treatment and resource recovery of waste ternary lithium batteries.
[0050] In step S6, before the positive electrode and the negative electrode are crushed, the following treatment is also included: the positive electrode and the negative electrode are placed in an infrared drying oven respectively, and dried at 170° C. for 30 minutes to ensure that the electrolyte can be completely removed.
[0051] In this embodiment, the effects of different vent hole diameters, different vent hole opening positions, and different vent hole numbers on the removal of electrolyte and powder in waste ternary lithium batteries are also investigated, as shown in Table 1-3.
[0052] Table 1 Comparison of the removal effects of different vent hole diameters on electrolyte and powder in waste ternary lithium batteries in Example 1
[0053]
[0054] In Table 1, except for the different diameters of the exhaust holes, other conditions are the same as those in Example 1; meanwhile, the electrolyte removal rate refers to the percentage of the electrolyte in the total mass of the battery. Generally speaking, the electrolyte in a lithium-ion battery accounts for 10%-15% of the mass of the entire battery.
[0055] It can be seen from Table 1 that when the aperture of the vent hole is 4mm, 5mm, and 6mm, the removal rate of the electrolyte is 9.7%, 10.47%, and 12.58%, respectively. It can be seen that when the aperture of the vent hole is 4mm to 6mm, the electrolyte in the battery can be effectively removed. In particular, when the aperture of the vent hole is 6mm, the electrolyte in the battery has been completely removed. At the same time, it can be seen from Table 1 that when the aperture of the vent hole is 2mm or 10mm, it is difficult to effectively remove the electrolyte in the battery. Their removal rates of the electrolyte in the battery are 4% and 6.2%, respectively. This shows that when the aperture of the vent hole is small or large, it is not conducive to improving the removal effect of the electrolyte. In particular, when the aperture of the vent hole is too large, there is still a risk of electrolyte leakage.
[0056] Table 2 Comparison of the removal effects of different opening positions on electrolyte and powder in waste ternary lithium batteries in Example 1
[0057]
[0058] In Table 2, except for the different opening positions of the exhaust holes, other conditions are the same as those in Example 1.
[0059] It can be seen from Table 2 that when the opening position of the vent hole is located near one end of the electrode, the removal effect of the electrolyte in the battery is the best. Although the opening position of the vent hole is in the middle of the battery or far away from the electrode end, the electrolyte in the battery can also be effectively removed, but such a hole opening method is prone to cause a large amount of powder loss. The reason may be: when punching holes in the middle of the battery or the outer shell far away from the motor end, it is easy to damage the inner core of the battery, causing the powder to be discharged outward with the electrolytic gas. In particular, when the opening position of the vent hole is located in the middle of the battery, since the diaphragm and the outer shell are attached together, when the gas pressure in the battery increases, it is also easy for the diaphragm to block the vent hole, so that the battery is prone to bulging during the infrared evaporation process.
[0060] Table 3 Comparison of the removal effects of different numbers of vent holes on electrolyte and powder in waste ternary lithium batteries in Example 1
[0061]
[0062] In Table 3, except for the number of exhaust holes and the distance between two holes, other conditions are the same as those in Example 1, wherein the distance between the exhaust holes is adaptively adjusted according to actual conditions.
[0063] It can be seen from Table 3 that when the number of exhaust holes on the battery surface is 3, 6, 9, and 12, the removal effect of the electrolyte in the battery is better. In particular, when the number of exhaust holes is 9, the electrolyte in the battery can be completely removed. At the same time, it can be seen from Table 3 that when the number of exhaust holes on the battery surface is 1 or 3, the exhaust holes are easily blocked, which may be the reason for the relatively poorer electrolyte removal effect. In addition, although the electrode liquid in the battery can be effectively removed when the number of exhaust holes on the battery surface is 12, the evaporation efficiency of the electrolyte is very low under this condition. This is mainly because the excessive number is not conducive to increasing the pressure in the battery, making it difficult to promote the discharge of the electrolytic gas in the battery.
[0064] In this embodiment, the influence of different infrared evaporation temperatures on the components in the waste ternary lithium battery is also investigated, as shown in Table 4.
[0065] Table 4 Effects of different infrared evaporation temperatures on the components of waste ternary lithium batteries in Example 1
[0066]
[0067] In Table 4, except for the infrared evaporation temperature, other conditions are the same as those in Example 1. The rotary kiln heating is to put the waste ternary lithium battery after needle puncture into a rotary kiln and dry it at 500°C.
[0068] As shown in Table 4, when the infrared evaporation temperature is 100°C, the removal effect of the electrolyte in the battery is poor. The reason may be that it is difficult to vaporize the electrolyte at a temperature of 100°C. When the temperature rises to 120°C-140°C, the removal rate of the electrolyte in the battery is significantly improved, reaching 9.8%-12.58%, and the electrolyte in the battery can be basically completely removed. At the same time, under this temperature condition, it will not have an adverse effect on the positive electrode sheet, negative electrode sheet, diaphragm and other components in the battery. However, when the temperature rises to 160°C, although the electrolyte in the battery can be completely removed, it also makes the positive electrode sheet brittle and the diaphragm melt, and finally forms a jelly, which makes it difficult to effectively separate the various raw materials. In addition, although the conventional rotary kiln heating method can also effectively remove the electrolyte in the battery, it also has the disadvantages of large powder loss, brittleness of the positive electrode sheets, sticking of the negative electrode sheets together, and melting or partial carbonization of the diaphragm. This not only increases the difficulty of separating the various raw materials, but also makes it difficult to obtain high-purity and high-recovery products.
[0069] In this embodiment, the influence of different infrared evaporation temperatures on the recovery effect of each component in the waste ternary lithium battery is also investigated, as shown in Table 5.
[0070] Table 5 Effect of different infrared evaporation temperatures on the recovery rate of each recovered component and product purity in Example 1
[0071]
[0072] In Table 5, except for the infrared evaporation temperature, other conditions are the same as those in Example 1. The rotary kiln heating is to put the waste ternary lithium battery after needle puncture into a rotary kiln and dry it at 500°C.
[0073] As can be seen from Table 5, when the infrared evaporation temperature is 100°C, the removal effect of the electrolyte is poor, so it is necessary to continue the infrared evaporation treatment. When the temperature rises to 120-140°C, positive electrode material powder and negative electrode material powder with high recovery rate and high purity can be obtained, which also shows that: under this temperature condition, there will be no adverse effects on the positive electrode sheet, negative electrode sheet, diaphragm and other components in the battery. Further, when the temperature rises to 160°C, the recovery rate and purity of the positive electrode material powder and the negative electrode material powder are reduced. The reason may be that under this temperature condition, the positive electrode sheet becomes brittle, the diaphragm melts, and forms a colloid, which makes it difficult to separate the positive and negative electrode sheet powders and diaphragm materials from the positive and negative active materials, and ultimately leads to poor recovery rate and purity. In addition, compared with the conventional rotary kiln heating method, the present invention adopts an overall drying method combining drilling and infrared evaporation, which will not destroy the original components and structure of the battery, and is conducive to the separate separation of each component in the subsequent process. It has high separation efficiency, high recovery volume, and high product purity. While achieving the separate separation of each useful component, higher quality products can also be obtained, which is ultimately conducive to the harmless treatment and resource processing of waste lithium-ion batteries.
[0074] Comparative Example 1
[0075] A method for treating and recycling waste lithium-ion batteries is basically the same as Example 1, with the only difference being that in Example 1, the safety valve of the waste ternary lithium battery is broken after acupuncture.
[0076] Comparative Example 2
[0077] A method for processing and recycling waste lithium-ion batteries is basically the same as Example 1, with the only difference being that in Comparative Example 2, after acupuncture, the top cover of the waste ternary lithium battery is cut off.
[0078] Table 6 Effects of different treatment methods in Example 1 and Comparative Examples 1-2 on the components of waste ternary lithium batteries
[0079]
[0080] As shown in Table 6, whether the safety cover or the top cover is removed, infrared radiation cannot be used to effectively remove the electrolyte in the battery. At the same time, the above-mentioned treatment method still has the disadvantages of large powder loss, embrittlement of the positive electrode sheet, and melting of the diaphragm. Completely different from them, in Example 1 of the present invention, under the condition that there is no need to open the safety cover or remove the top cover, the overall drying method of punching combined with infrared evaporation is adopted, which is not only more conducive to the efficient removal of the electrolyte in the battery, but also does not destroy the original components and original structure of the battery. In particular, only through the process of reverse winding, crushing and other processes, higher quality products can be obtained while realizing the separation of each useful component, which is convenient for realizing the batch processing of waste lithium-ion batteries, and has an important role in promoting the harmless treatment and resource utilization of more waste lithium-ion batteries.
[0081] It can be seen from the above results that, compared with conventional treatment methods, the treatment and resource recovery method of waste lithium-ion batteries of the present invention has the following advantages: (a) higher safety; (b) higher efficiency; (c) more energy-saving; (d) more environmentally friendly; (e) lower cost. Therefore, the treatment and resource recovery method of waste lithium-ion batteries of the present invention has the advantages of high safety factor, high treatment efficiency, low energy consumption, low cost, high product recovery rate, high product purity, good economic benefits, etc., can realize batch treatment of waste lithium-ion batteries, and can also recover a large amount of high-value positive and negative electrode materials from waste lithium-ion batteries, with high use value and good application prospects.
[0082] The above embodiments are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for processing and recycling waste lithium-ion batteries, It is characterized in that The following steps are involved: S1. Discharging the waste lithium-ion batteries; S2, punching holes in the outer shell of the waste lithium-ion battery after the discharge treatment to form exhaust holes on one side of the waste lithium-ion battery; the diameter of the exhaust holes is 4 mm to 6 mm; the exhaust holes are located on the surface of one end of the electrode of the waste lithium-ion battery; the number of the exhaust holes is 6 to 9; S3, with the exhaust hole facing upward, performing infrared evaporation on the waste lithium-ion battery to remove the electrolyte in the waste lithium-ion battery; the infrared evaporation is performed at a temperature of 120° C. to 140° C.; S4, dismantling the waste lithium-ion batteries after infrared evaporation and taking out the battery cells; S5, reversely winding the battery cell to obtain a positive electrode, a negative electrode and a separator; S6. The positive electrode and the negative electrode are crushed respectively to obtain positive electrode material powder, negative electrode material powder, aluminum powder and copper powder, thereby completing the treatment and resource recovery of waste lithium-ion batteries.
2. The method for processing and recycling waste lithium-ion batteries according to claim 1, It is characterized in that The distance between the exhaust hole and the edge close to one end of the electrode of the waste lithium-ion battery is ≤10mm; The exhaust holes are distributed in a row on the surface close to one end of the electrode of the waste lithium-ion battery, and the distance between every two exhaust holes is 10 mm to 30 mm.
3. The method for processing and recycling waste lithium-ion batteries according to claim 2, It is characterized in that In step S2, the outer shell of the waste lithium-ion battery after the discharge treatment is punched by acupuncture; the depth of the exhaust hole is the same as the thickness of the outer shell.
4. The method for processing and recycling waste lithium-ion batteries according to claim 3, It is characterized in that In step S3, infrared radiation is used to perform infrared evaporation on the waste lithium-ion batteries, so that the electrolyte in the waste lithium-ion batteries is vaporized and discharged from the exhaust holes; the wavelength of the infrared radiation is 5 μm to 25 μm; and the time of the infrared evaporation is 75 min to 90 min.
5. The method for processing and recycling waste lithium-ion batteries according to claim 4, It is characterized in that An infrared heating plate is used as an infrared radiation source to perform infrared evaporation on waste lithium-ion batteries; the infrared heating plate is located above the waste lithium-ion batteries, and / or the infrared heating plate is located below the waste lithium-ion batteries, and / or the infrared heating plate is located on the side of the waste lithium-ion batteries; the infrared heating plate includes a thermal insulation layer, an infrared heating layer and a heat-conducting layer stacked in sequence from bottom to top; the infrared heating layer is a graphene heating layer, and the graphene heating layer is bonded to the heat-conducting layer; the heat-conducting layer is a microcrystalline glass plate.
6. The method for treating and recycling waste lithium-ion batteries according to any one of claims 1 to 5, It is characterized in that In step S1, the waste lithium-ion batteries include lithium iron phosphate batteries and / or ternary lithium batteries.
7. The method for treating and recycling waste lithium-ion batteries according to any one of claims 1 to 5, It is characterized in that Step S3 also includes the following processes: collecting tail gas generated during the infrared evaporation process; burning the tail gas using plasma combustion technology; The waste gas generated during the combustion process is discharged after dust removal.
8. The method for treating and recycling waste lithium-ion batteries according to any one of claims 1 to 5, It is characterized in that In step S5, the subsequent treatment of the diaphragm includes the following steps: burning the diaphragm; and exhausting the waste gas generated during the burning process after dust removal.
9. The method for treating and recycling waste lithium-ion batteries according to any one of claims 1 to 5, It is characterized in that In step S6, before the positive electrode and the negative electrode are crushed, the following treatment is also included: the positive electrode and the negative electrode are dried respectively in an infrared drying furnace; the drying temperature is 170° C. to 210° C.; the drying time is 30 min to 60 min.
Citation Information
Patent Citations
Method for comprehensive harmless recovery and utilization of waste lithium ion power battery
CN105428745A
Comprehensive utilization method for waste lithium ion batteries
CN105958150A
Device and method for extracting electrolyte liquid of spent lithium-ion batteries
CN108270046A
Method for inactivating waste electrified soft package lithium ion battery before crushing
CN111029677A
Lithium iron phosphate battery positive electrode material recovery device
CN219626730U