Lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder and preparation method thereof

The preparation of lanthanum bismuth doped tin oxide nano powders through ball mill dispersion and airflow crushing technology, solving the problem of water-soluble impurities in the hydrothermal method, achieving efficient and environmentally friendly production of near-infrared reflective materials, with good transparency and thermal insulation effect .

CN118666308BActive Publication Date: 2024-11-26CHANGDI NEW MATERIAL TECHNOLOGY (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411147341.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

When preparing near-infrared reflective materials with existing hydrothermal methods, a large number of water-soluble impurities are generated, which is cumbersome and is not conducive to industrial production. It requires separation and washing steps, which affects environmental protection.

Method used

The ball mill dispersion and airflow crushing technology are used to prepare lanthanum bismuth doped tin oxide near-infrared reflective nanopowder. By mixing ethanol with mixed powder and grinding of spherical zirconium beads, the initial particle size and particle size distribution are reduced, agglomeration is reduced, and washing is avoided. The separation step is to protect the sintering with inert gas.

Benefits of technology

The high transmittance and near-infrared reflectivity of lanthanum bismuth doped tin oxide nano powder are achieved, with narrow particle size distribution and high uniformity, which simplifies production processes, saves energy, and improves industrial applicability and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118666308B_ABST
    Figure CN118666308B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of near-infrared reflective materials, and specifically discloses a lanthanum bismuth doped tin oxide near-infrared reflective nanopowder and a preparation method thereof. A preparation method of lanthanum bismuth doped tin oxide near-infrared reflective nanopowder comprises: stirring and mixing tin oxide and a dopant to obtain a mixed powder; mixing the mixed powder and ethanol, ball milling and dispersing the mixed powder, and then drying to obtain a ball milled and dispersed mixed powder; air flow crushing the ball milled and dispersed mixed powder, and then sintering it under the protection of an inert gas, and finally crushing it to obtain lanthanum bismuth doped tin oxide near-infrared reflective nanopowder; the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder prepared by the solid phase method in the present application does not introduce impurities such as chloride salts, so it does not need to be washed and wastewater treated, which saves energy and improves the applicability of industrial production of lanthanum bismuth doped tin oxide near-infrared reflective nanopowder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of near-infrared reflective materials, and more specifically, to a lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder and a preparation method thereof. Background Art

[0002] Near-infrared reflective material is a material that can reflect light in the near-infrared region. It can effectively reflect sunlight and reduce heat absorption, thereby achieving a heat insulation effect.

[0003] The hydrothermal method is a method that uses a high-pressure, high-temperature water environment to carry out chemical reactions. The hydrothermal method usually uses oxides or hydroxides as precursors and water as the reaction medium. The mixture of the precursor and water is first subjected to a hydrothermal reaction under high temperature and high pressure conditions, and then subjected to post-processing such as separation, washing, and drying to obtain a powder material. Since the powder obtained by the hydrothermal method has the characteristics of complete grain development, small particle size, and uniform distribution, the hydrothermal method is currently commonly used to prepare near-infrared reflective materials.

[0004] However, during the hydrothermal reaction of the mixture of precursor and water, a large amount of water-soluble impurities will be generated after the precursor is dissolved. Although most of the water-soluble impurities can be removed by multiple washings, the operation is cumbersome and a large amount of wastewater will be generated, which is not conducive to industrial production. Summary of the invention

[0005] In order to improve the applicability of near-infrared reflective materials for industrial production, the present application provides a lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder and a preparation method thereof.

[0006] In a first aspect, the present application provides a method for preparing lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder, using the following technical solution:

[0007] A method for preparing lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder comprises the following preparation steps:

[0008] S1: Stirring and mixing tin oxide and a dopant to obtain a mixed powder;

[0009] S2: mixing the mixed powder and ethanol, performing ball milling dispersion, and then drying to obtain a ball milled and dispersed mixed powder;

[0010] The ball milling dispersion time is 5 to 24 hours, the main wheel revolution speed is 270 to 320 r / min, the grinding jar rotation speed is 557 to 660 r / min, the motor power is 0.75 kW, and the grinding medium is spherical 95 zirconium beads with a size of 0.08 to 0.13 mm;

[0011] S3: airflow crushing the mixed powder dispersed by ball milling, sintering under the protection of inert gas, and finally crushing to obtain lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder;

[0012] The pressure of air flow crushing is 0.1~1MPa, and the time is 0.5~5h;

[0013] The dopants include bismuth oxide and lanthanum oxide.

[0014] Tin oxide powder is a transparent oxide with good transparency. By adopting the above technical solution, the mixed powder is mixed with highly polar ethanol to promote the dispersion of the mixed powder, reduce its agglomeration, and facilitate the ball milling shearing of zirconium beads of specific shapes and sizes, thereby reducing the particle size of the mixed powder after ball milling dispersion. Subsequently, under the condition of a pressure of 0.1 to 1 MPa, the mixed powder after ball milling dispersion is crushed by air flow for 0.5 to 5 hours, which can reduce the particle size distribution of the mixed powder before sintering, and is conducive to obtaining lanthanum and bismuth doped tin oxide powder with a narrow particle size distribution after sintering. Finally, the powder is crushed again, which can effectively reduce the agglomeration of the powder and further improve the uniformity of the powder particles.

[0015] Therefore, the present application adopts ball milling dispersion and air flow crushing technology to make the initial particle size of the mixed raw materials smaller and narrower, so that lanthanum and bismuth with near-infrared reflection function are uniformly doped into the tin oxide lattice, and the advantages of high transmittance, high near-infrared reflection function, small particle size, narrow particle size distribution and not easy to agglomerate are obtained. Compared with the preparation of nanopowders by hydrothermal method, the preparation method of the present application does not use raw materials such as chloride salts, so there is no need for post-processing steps such as separation and washing, which is easy to operate, avoids residual chloride ions, and does not waste water resources. It is more environmentally friendly and improves the applicability of near-infrared reflection nanopowders for industrial production.

[0016] Preferably, the dopant is composed of bismuth oxide and lanthanum oxide mixed in a weight ratio of 1:(0.006-0.350).

[0017] By adopting the above technical solution, lanthanum and bismuth are co-doped with tin oxide, and the prepared nanopowder has a higher near-infrared reflectivity. At the same time, compared with bismuth doped tin oxide, lanthanum and bismuth co-doped tin oxide makes the powder less agglomerated after sintering, with a smaller particle size and more uniform distribution.

[0018] Preferably, the tin oxide and the dopant are mixed in a weight ratio of 1:(0.003-0.033).

[0019] By adopting the above technical solution, the proportion of dopants in tin oxide is optimized, which is conducive to obtaining nanopowders with both high transmittance and high near-infrared reflectivity. The nanopowder can be used in window films or architectural films and has good transparency and heat insulation effects.

[0020] Preferably, the mixed powder and ethanol are mixed in a weight ratio of 1:(2-5).

[0021] By adopting the above technical solution, the mixed powder can be fully dispersed by adding an appropriate amount of ethanol, which promotes the collision of zirconium beads and mixed powder. This can not only reduce the particle size of the obtained nanopowder and reduce powder agglomeration, but also reduce costs and improve the applicability of nanopowder for industrial production.

[0022] Preferably, the drying temperature is 80-90° C. and the drying time is 2-6 hours.

[0023] By adopting the above technical scheme, the mixed powder and ethanol after ball milling dispersion are dried at a temperature slightly higher than the boiling point of ethanol, so that the ethanol in the mixed powder is gradually volatilized, the hydrogen bonding effect between the mixed powders is reduced, and the formation of bridging oxygen bonds between the mixed powders is alleviated, thereby reducing the agglomeration of the mixed powder and improving the uniformity of the obtained nanopowder.

[0024] Preferably, the sintering temperature is 800-1200° C., and the sintering time is 3-10 hours.

[0025] Preferably, the inert gas is nitrogen or argon or a mixture of argon and hydrogen.

[0026] By adopting the above technical scheme, under the protection of inert gas, the mixed powder is sintered at 800-1200°C after airflow crushing, which not only facilitates the doping of lanthanum and bismuth into the tin oxide lattice to obtain a nano powder with a rutile phase structure, but also the obtained nano powder still has high activity and a small particle size.

[0027] Preferably, the rotation speed of the pulverization is 2000-15000 r / min.

[0028] By adopting the above technical solution, the sintered powder is crushed at a rotation speed of 2000-15000 r / min, which can reduce the agglomeration of nano powder and improve the uniformity of the particle size of the nano powder.

[0029] Preferably, S2 comprises the following steps:

[0030] S21: stirring and mixing the mixed powder and ethanol with a mass fraction of 30-40%, stirring and mixing at 65-70° C. for 1-2 hours, and then drying under reduced pressure to obtain a dried mixed powder;

[0031] S22: After the dried mixed powder is stirred and mixed with ethanol having a mass fraction of 25 to 35%, it is first ball-milled and dispersed for 1 to 3 hours, and then the remaining ethanol is added, ball-milled and dispersed for 4 to 21 hours, and dried to obtain a mixed powder after ball-milling dispersion.

[0032] By adopting the above technical scheme, part of the ethanol and the mixed powder are first premixed and dried at a specific temperature. The highly polar ethanol can quickly penetrate and disperse the mixed powder. On the one hand, it can dissolve and remove impurities on the surface of the mixed powder, thereby improving the purity of the obtained nano powder; on the other hand, by adding low-boiling-point ethanol, the boiling point of the mixture of the mixed powder and ethanol can be reduced, which is convenient for reducing the pressure and drying to remove the moisture in the mixed powder, thereby reducing the hydrogen bonding between the mixed powders, improving the agglomeration of the nano powders, and improving the uniformity of the particle size of the nano powders.

[0033] At the same time, when ethanol is mixed with the premixed and dried mixed powders in batches, the interaction between the mixed powders and the zirconium beads will be more sufficient, which is beneficial to improving the grinding efficiency and reducing the particle size of the nanopowders.

[0034] In a second aspect, the present application provides a lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder, which adopts the following technical solution:

[0035] A lanthanum-bismuth-doped tin oxide near-infrared reflecting nano powder is prepared by the preparation method of the lanthanum-bismuth-doped tin oxide near-infrared reflecting nano powder.

[0036] By adopting the above technical solution and the above preparation method, lanthanum and bismuth having near-infrared reflection function are co-doped with tin oxide, and the obtained nanopowder not only has high transmittance and near-infrared reflectivity, but also has a narrow particle size distribution and higher uniformity.

[0037] In summary, this application has the following beneficial effects:

[0038] 1. Since the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder prepared by the solid phase method in the present application does not introduce impurities such as chloride salts, washing and wastewater treatment are not required, which saves energy and improves the applicability of lanthanum bismuth doped tin oxide near-infrared reflective nanopowder for industrial production;

[0039] 2. The present application reduces the initial particle size of the mixed powder by ball milling and air flow pulverization, making its particle size distribution narrower, and making the mixed doping of lanthanum and bismuth more uniform. The nanopowder obtained after sintering has less agglomeration and a narrower particle size distribution;

[0040] 3. The lanthanum bismuth doped tin oxide near-infrared reflective nanopowder of the present application has both high transmittance and near-infrared reflectivity, can be used in car window films or building films, and has good light transmission and heat insulation effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the XRD diagram of the lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder of Example 1 of the present application;

[0042] Figure 2 This is a normal distribution diagram of the particle size of the lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder of Example 1 of the present application;

[0043] Figure 3 It is a normal distribution diagram of the particle size of the nano powder in comparative example 3 of the present application. DETAILED DESCRIPTION

[0044] The present application is further described in detail below with reference to the accompanying drawings and embodiments.

[0045] The raw materials used in the examples of the present application are commercially available unless otherwise specified below.

[0046] The purity of tin oxide powder is 99.9%, and the average particle size is 1um;

[0047] The purity of lanthanum oxide powder is 99.99%, and the average particle size is 1um;

[0048] The purity of bismuth oxide powder is 99.9%, and the average particle size is 1um;

[0049] Planetary ball mill, main wheel revolution speed 45 ~ 435r / min, grinding tank rotation speed 90 ~ 870r / min, motor power is 0.75kW, grinding medium is spherical 95 zirconium beads, size 0.08 ~ 0.13mm;

[0050] The air flow pulverizer is an ultra-fine air flow pulverizer with a main shaft speed of 4000r / min and a motor power of 15kW.

[0051] Performance Testing

[0052] The particle size, light transmittance and near-infrared reflectivity of the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder prepared in the example of the present application and the nanopowder prepared in the comparative example were tested, and the testing method was as follows:

[0053] 1. Particle size detection

[0054] Preparation of the sample to be tested: Take 0.1 g of lanthanum bismuth doped tin oxide near-infrared reflective nanopowder or nanopowder and add it to 30 ml of anhydrous ethanol, and ultrasonicate for 10 minutes to obtain the sample to be tested.

[0055] Blank sample preparation: 30 ml of anhydrous ethanol.

[0056] Detection: Use a laser particle size analyzer. After the blank determination is completed, add a drop of the above sample to be tested, observe whether the window curve appears, add drop by drop until the particle size distribution curve is stable, and then start testing to obtain the particle size distribution.

[0057] 2. Light transmittance and near-infrared reflectivity testing

[0058] Nanopowder to be tested: prepared lanthanum bismuth doped tin oxide near-infrared reflective nanopowder or nanopowder.

[0059] Preparation of test film: 16 g of the prepared nanopowder and 1 kg of crushed PET particles were weighed and blended, extruded and cast into a film at 260° C. using a twin-screw extruder, and then biaxially stretched into a film with a thickness of 19 μm to obtain the test film.

[0060] Light transmittance: Refer to GB / T 5137.2-2020 Test methods for automotive safety glass, Part 2: Optical properties test, use Shimadzu UV-Vis-NIR spectrophotometer UV-3600 to test, and record the visible light transmittance at 550nm.

[0061] Near-infrared reflectivity: Refer to GB / T 5137.4-2020 Test methods for automotive safety glass, Part 4: Solar properties test, use Shimadzu UV-Vis-NIR spectrophotometer UV-3600 to test, and record the near-infrared reflectivity at 950nm and 1400nm.

[0062] Example 1

[0063] A lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder, the raw materials and their corresponding weights (g) are shown in the following table.

[0064]

[0065] The preparation method of the above-mentioned lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder comprises the following preparation steps:

[0066] S1: Stirring and mixing tin oxide and a dopant to obtain a mixed powder;

[0067] S2: After mixing the mixed powder and ethanol, first add them into a planetary ball mill for ball milling dispersion, and then dry them to obtain a mixed powder after ball milling dispersion;

[0068] In the planetary ball mill, the main wheel revolution speed is 320r / min, the grinding jar rotation speed is 660r / min, the motor power is 0.75kW, the grinding medium is spherical 95 zirconium beads with a size of 0.08-0.13mm, the ball milling dispersion time is 6h; the drying temperature is 80℃, and the time is 3h;

[0069] S3: firstly, the mixed powder after ball milling is added into a jet mill for jet milling, then added into a tubular furnace for sintering under the protection of inert gas, and finally added into a mill for milling to obtain lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder;

[0070] The pressure of air flow crushing is 0.8MPa and the time is 1h;

[0071] The sintering temperature is 1000°C and the time is 3h;

[0072] The crushing speed is 3000r / min.

[0073] Example 2

[0074] A lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder, the raw materials and their corresponding weights (g) are shown in the following table.

[0075]

[0076] The preparation method of the above-mentioned lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder comprises the following preparation steps:

[0077] S1: Stirring and mixing tin oxide and a dopant to obtain a mixed powder;

[0078] S2: After mixing the mixed powder and ethanol, first add them into a planetary ball mill for ball milling dispersion, and then dry them to obtain a mixed powder after ball milling dispersion;

[0079] In the planetary ball mill, the main wheel revolution speed is 270r / min, the grinding jar rotation speed is 557r / min, the motor power is 0.75kW, the grinding medium is spherical 95 zirconium beads with a size of 0.08-0.13mm, the ball milling dispersion time is 8h; the drying temperature is 80℃, and the time is 4h;

[0080] S3: firstly, the mixed powder after ball milling is added into a jet mill for jet milling, then added into a tubular furnace for sintering under the protection of inert gas, and finally added into a mill for milling to obtain lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder;

[0081] The pressure of air flow crushing was 0.7 MPa and the time was 2 h;

[0082] The sintering temperature is 900°C and the time is 5h;

[0083] The crushing speed is 6500r / min.

[0084] Example 3

[0085] A lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder, the raw materials and their corresponding weights (g) are shown in the following table.

[0086]

[0087] The preparation method of the above-mentioned lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder comprises the following preparation steps:

[0088] S1: Stirring and mixing tin oxide and a dopant to obtain a mixed powder;

[0089] S2: After mixing the mixed powder and ethanol, first add them into a planetary ball mill for ball milling dispersion, and then dry them to obtain a mixed powder after ball milling dispersion;

[0090] In the planetary ball mill, the main wheel revolution speed is 300r / min, the grinding jar rotation speed is 620r / min, the motor power is 0.75kW, the grinding medium is spherical 95 zirconium beads with a size of 0.08-0.13mm, the ball milling dispersion time is 7h; the drying temperature is 80℃, and the time is 3.5h;

[0091] S3: firstly, the mixed powder after ball milling is added into a jet mill for jet milling, then added into a tubular furnace for sintering under the protection of inert gas, and finally added into a mill for milling to obtain lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder;

[0092] The pressure of air flow crushing is 0.7MPa and the time is 0.5h;

[0093] The sintering temperature is 950°C and the sintering time is 6h;

[0094] The crushing speed is 4000r / min.

[0095] The light transmittance, near-infrared reflectivity and particle size of the lanthanum bismuth doped tin oxide near-infrared reflective nanopowders prepared in Examples 1 to 3 of the present application were tested, and the test results are shown in the following table.

[0096]

[0097] Depend on Figure 1 It can be seen that in Example 1, lanthanum and bismuth are doped into the tin oxide lattice, and the rutile phase structure is still present. Figure 2 It can be seen that the particle size of Example 1 is small and the distribution is narrow.

[0098] By analyzing the data in the above table, it can be seen that the film prepared by using the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder of Examples 1 to 3 of the present application has a light transmittance of up to 75-80%, a near-infrared reflectivity of up to 39-42.31% at 950nm, and a near-infrared reflectivity of up to 50.2-55.0% at 1400nm. This shows that the film prepared by using the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder of Examples 1 to 3 of the present application has excellent light transmission and heat insulation effects.

[0099] At the same time, the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder prepared in Examples 1 to 3 of the present application has a particle size as low as 0.069 to 0.140 nm at D50, and a particle size range as low as 0.033 to 0.458 nm at D10 to D90. This shows that the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder prepared in Examples 1 to 3 of the present application has a lower particle size and a narrower particle size range.

[0100] In particular, in Example 3, the particle size at D50 is as low as 0.069 nm, and the particle size range at D10 to D90 is as low as 0.0330 to 0.122 nm.

[0101] Example 4

[0102] A lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, which is different from Example 3 in that the preparation method of the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder comprises the following preparation steps:

[0103] S1: Stir and mix tin oxide and a dopant to obtain a mixed powder.

[0104] S2:

[0105] S21: firstly, the mixed powder and 35% by mass ethanol are stirred and mixed, and then stirred and mixed at 68° C. for 1.5 h, and then dried under reduced pressure to obtain a dried mixed powder;

[0106] S22: After the dried mixed powder and 30% by mass ethanol are stirred and mixed, the mixture is first added into a planetary ball mill for ball milling dispersion for 2.5 hours, and then the remaining ethanol is added, the mixture is ball milled and dispersed for 4.5 hours, and dried to obtain a mixed powder after ball milling dispersion;

[0107] The drying temperature is 80°C and the drying time is 3.5 hours.

[0108] S3: firstly, the mixed powder after ball milling is added into a jet mill for jet milling, then added into a tubular furnace for sintering under the protection of inert gas, and finally added into a mill for milling to obtain lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder;

[0109] The pressure of air flow crushing is 0.7MPa and the time is 0.5h;

[0110] The sintering temperature is 950°C and the sintering time is 6h;

[0111] The crushing speed is 4000r / min.

[0112] Example 5

[0113] A lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, which is different from Example 3 in that in the preparation method of the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, steps S21 and S22 are:

[0114] S21: After the mixed powder and 30% by mass ethanol are stirred and mixed, the mixture is stirred and mixed at 65° C. for 2 h, and then dried under reduced pressure to obtain a dried mixed powder;

[0115] The drying temperature is 80°C and the drying time is 3.5 hours.

[0116] S22: After the dried mixed powder is stirred and mixed with ethanol having a mass fraction of 25%, it is first added into a planetary ball mill for ball milling dispersion for 3 hours, and then the remaining ethanol is added, ball milling dispersion is performed for 4 hours, and dried to obtain a mixed powder after ball milling dispersion.

[0117] Example 6

[0118] A lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, which is different from Example 3 in that in the preparation method of the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, steps S21 and S22 are:

[0119] S21: stirring the mixed powder and 40% by mass ethanol, stirring and mixing at 70° C. for 1 hour, and then drying under reduced pressure to obtain a dried mixed powder;

[0120] The drying temperature is 80°C and the drying time is 3.5 hours.

[0121] S22: After the dried mixed powder is stirred and mixed with 35% by mass ethanol, it is first added into a planetary ball mill for ball milling dispersion for 2 hours, and then the remaining ethanol is added, ball milling dispersion is performed for 5 hours, and dried to obtain the mixed powder after ball milling dispersion.

[0122] Example 7

[0123] A lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, which is different from Example 3 in that in the preparation method of the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, steps S21 and S22 are:

[0124] S21: After the mixed powder and ethanol with a mass fraction of 25% are stirred and mixed, the mixture is stirred and mixed at 60° C. for 1.5 h, and then dried under reduced pressure to obtain a dried mixed powder;

[0125] The drying temperature is 80°C and the drying time is 3.5 hours.

[0126] S22: After the dried mixed powder is stirred and mixed with ethanol having a mass fraction of 25%, it is first added into a planetary ball mill for ball milling dispersion for 1 hour, and then the remaining ethanol is added, ball milling dispersion is performed for 6 hours, and dried to obtain a mixed powder after ball milling dispersion.

[0127] Example 8

[0128] A lanthanum bismuth doped tin oxide near-infrared reflective nanopowder, which is different from Example 3 in that the preparation method S2 of the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder includes the following preparation steps:

[0129] S21: After the mixed powder and 45% by mass ethanol are stirred and mixed, the mixture is stirred and mixed at 75° C. for 1.5 h, and then dried under reduced pressure to obtain a dried mixed powder;

[0130] The drying temperature is 80°C and the drying time is 3.5 hours.

[0131] S22: After the dried mixed powder is stirred and mixed with 40% by mass ethanol, it is first added into a planetary ball mill for ball milling dispersion for 5 hours, and then the remaining ethanol is added, ball milling dispersion is performed for 2 hours, and dried to obtain the mixed powder after ball milling dispersion.

[0132] The particle size of the lanthanum and bismuth doped tin oxide near-infrared reflective nanopowders prepared in Examples 4 to 8 of the present application was tested, and the test results are shown in the following table.

[0133]

[0134] By analyzing the data in the above table, it can be seen that the lanthanum bismuth doped tin oxide near-infrared reflective nanopowders prepared in Examples 4 to 6 of the present application have a particle size as low as 0.064 to 0.058 nm at D50, and a particle size range as low as 0.0310 to 0.117 nm at D10 to D90.

[0135] Compared with Example 3, Examples 4 to 6 have a smaller particle size at D50, and a narrower particle size range at D10 to D90. This shows that in the preparation method of lanthanum bismuth doped tin oxide near-infrared reflective nanopowder of the present application, part of ethanol and mixed powder are first premixed and dried at a specific temperature. Since the highly polar ethanol can quickly penetrate and disperse the mixed powder, dissolve and remove impurities on the surface of the mixed powder, and remove moisture from the mixed powder, the hydrogen bonding between the mixed powders is reduced, the agglomeration of the nanopowder is improved, and the uniformity of the nanopowder particle size is improved.

[0136] Compared with Examples 4 to 6, the particle size of Examples 7 and 8 at D50 is larger, and the particle size range at D10 to D90 is wider. This shows that in the preparation method of lanthanum bismuth doped tin oxide near-infrared reflective nanopowder of the present application, by controlling the amount of ethanol used during premixing and drying, and the time of step-by-step ball milling, the particle size at D50 can be reduced, and the particle size range at D10 to D90 can be reduced. Analysis shows that the reason may be that the amount of ethanol used during premixing is too much, and the amount of remaining ethanol during ball milling dispersion is small, and the mixed powder cannot be fully dispersed, resulting in insufficient grinding. However, the amount of ethanol used during premixing is too little, and the mixed powder is not fully dehydrated, so it will also affect the uniformity of the final nanopowder particle size.

[0137] Comparative Example 1

[0138] A nano powder, which is different from Example 3 in that an equal weight of bismuth oxide is used to replace lanthanum oxide.

[0139] Comparative Example 2

[0140] A nano powder, which is different from Example 3 in that an equal weight of butanone is used to replace ethanol.

[0141] Comparative Example 3

[0142] A nano powder, which is different from Example 3 in that, in the preparation method of lanthanum bismuth doped tin oxide near-infrared reflective nano powder, the ball milling dispersion time in S2 is 25 hours; the air flow crushing pressure in S3 is 1.5 MPa, and the time is 0.5 hours.

[0143] The light transmittance and near-infrared reflectivity of the nanopowder prepared in Comparative Example 1 of the present application were tested, and the particle size of the nanopowder prepared in Comparative Examples 2 to 3 was tested. The test results are shown in the following table.

[0144]

[0145] By analyzing the data in the above table, it can be seen that compared with the nanopowder prepared by doping bismuth oxide alone in Comparative Example 1, the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder prepared by co-doping bismuth oxide and lanthanum oxide in Example 3 has a smaller particle size and a narrower particle size range. This shows that in the total raw materials for preparing the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder of the present application, the use of bismuth oxide and lanthanum oxide co-doped tin oxide can reduce the particle size of the final prepared lanthanum bismuth doped tin oxide near-infrared reflective nanopowder and improve the uniformity of its particle size.

[0146] Compared with the nanopowder prepared by dispersing the mixed powder with butanone in Comparative Example 2, the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder prepared by dispersing the mixed powder with ethanol in Example 3 has a smaller particle size and a narrower particle size range. This shows that in the total raw materials for preparing the lanthanum bismuth doped tin oxide near-infrared reflective nanopowder of the present application, using ethanol to disperse the mixed powder can reduce the particle size of the final prepared lanthanum bismuth doped tin oxide near-infrared reflective nanopowder and improve the uniformity of its particle size.

[0147] Depend on Figure 3 It can be seen that the particle size of Comparative Example 3 is large and the distribution is wide. At the same time, compared with Example 3, although the ball milling dispersion time and the air flow crushing pressure are increased in the preparation method of Comparative Example 3. However, the particle size of Comparative Example 3 at D50 and the particle size range of D10 to D90 are still larger than those of Example 3. Analysis of the reason may be that, although long-term ball milling dispersion and large air flow crushing pressure can instantly reduce the particle size of nano powders, the specific surface area increases significantly after the particle size is reduced, and it is easier to agglomerate. Therefore, the present application can obtain nano powders with uniform particle size by optimizing the appropriate ball milling time and air flow crushing pressure.

[0148] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder, It is characterized in that The method comprises the following preparation steps: S1: Stirring and mixing tin oxide and a dopant to obtain a mixed powder; S2: mixing the mixed powder and ethanol, performing ball milling dispersion, and then drying to obtain a ball milled and dispersed mixed powder; The ball milling dispersion time is 5 to 24 hours; the main wheel disk revolution speed in the ball mill is 270 to 320 r / min, and the grinding jar rotation speed is 557 to 660 r / min; S3: airflow crushing the mixed powder dispersed by ball milling, sintering under the protection of inert gas, and finally crushing to obtain lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder; The pressure of air flow crushing is 0.1~1MPa, and the time is 0.5~5h; The rotation speed of the crushing is 2000-15000 r / min; The tin oxide and the dopant are mixed in a weight ratio of 1:(0.003-0.033); The dopant is composed of bismuth oxide and lanthanum oxide mixed in a weight ratio of 1:(0.006-0.350).

2. The method for preparing the lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder according to claim 1, It is characterized in that The mixed powder and ethanol are mixed in a weight ratio of 1:(2-5).

3. The method for preparing the lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder according to claim 1, It is characterized in that The drying temperature is 80-90° C. and the drying time is 2-6 hours.

4. The method for preparing the lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder according to claim 1, It is characterized in that The sintering temperature is 800-1200° C., and the sintering time is 3-10 hours.

5. The method for preparing the lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder according to claim 1, It is characterized in that The inert gas is nitrogen or argon or a mixed gas of argon and hydrogen.

6. The method for preparing the lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder according to claim 1, It is characterized in that The S2 comprises the following steps: S21: stirring and mixing the mixed powder and ethanol with a mass fraction of 30-40%, stirring and mixing at 65-70° C. for 1-2 hours, and then drying under reduced pressure to obtain a dried mixed powder; S22: After the dried mixed powder is stirred and mixed with ethanol having a mass fraction of 25 to 35%, it is first ball-milled and dispersed for 1 to 3 hours, and then the remaining ethanol is added, ball-milled and dispersed for 4 to 21 hours, and dried to obtain a mixed powder after ball-milling dispersion.

7. A lanthanum-bismuth-doped tin oxide near-infrared reflective nanopowder, It is characterized in that The powder is prepared by the method for preparing the lanthanum and bismuth doped tin oxide near-infrared reflective nanopowder according to any one of claims 1 to 6.