Silicone elastomer, gel, preparation method and application
By introducing branched structures and hydrophilic groups such as polyoxyalkylene ethers into the silicone elastomer, a silicone elastomer with excellent self-emulsification performance and stability is solved, and the lack of compatibility and difficulty in emulsification in the prior art is solved. The problem of oil production of products has achieved product stability and industrial adaptability.
Patent Information
- Application Number
- CN202411140681.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing silicone elastomers have problems such as insufficient compatibility, difficulty in emulsification, and easy oil production of products. The raw materials are not easy to obtain, high prices, and complex processes, which affect industrialization.
The cross-linking reaction is carried out by using Si-H polysiloxane with branched structure and unsaturated alkenyl polysiloxane. By introducing hydrophilic groups such as polyoxyalkylene ethers, silicone elastomers are formed, and their structure is excellent. Self-emulsification properties and stability.
It realizes the characteristics of silicone elastomers that are not easy to produce oil, have good compatibility and are easy to emulsify, reduces the oil yield of the product, improves the stability and compatibility of cosmetic formulas, and has a simple process and reasonable cost, which is suitable for industrial production. .
Smart Images

Figure CN118667167B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organosilicon elastomer polymer preparation, and in particular relates to an organosilicon elastomer, gel, preparation method and application. Background Art
[0002] Silicone elastomer (SE for short) refers to silicon-containing polymers with different network cross-linking structures. According to different states, it is mainly divided into three types: silicone elastomer gel, silicone elastomer powder, and silicone elastomer emulsion. It is widely used in personal care, textile industry, coating industry, construction, industry and other fields.
[0003] Among them, silicone elastomer gel (SEG for short) is a non-Newtonian fluid with shear-thinning properties. It is a mixture of cross-linked network-structured silicon-containing polymers swollen and diluted by diluents. It can give the skin a unique skin feel such as velvety lightness and silkiness, and is widely used in daily cosmetics such as sunscreen, makeup, and skin care.
[0004] Traditionally, the preparation of silicone elastomer gel mainly involves first preparing silicone elastomer, then mechanically shearing and crushing it, then diluting the gel by swelling, and finally dispersing and mixing it at high speed to obtain the uniform product. However, existing silicone elastomers have problems such as easy oiling, insufficient compatibility, and difficulty in emulsification. In order to solve the above problems, the industry has done a lot of research.
[0005] A Chinese invention patent application (publication number: CN104661645A, publication date: 2015-05-27) provides a copolymer having a carbosiloxane dendritic structure and a cosmetic composition containing the copolymer, which exhibits excellent compatibility with ultraviolet absorbers, and the cosmetics prepared therefrom have excellent water resistance, anti-sebum and stability. However, the process of the carbosiloxane dendritic structure copolymer is complex and costly, and multiple steps are required to achieve carbosiloxane dendronization, and there are many side reactions.
[0006] The Chinese invention patent application (publication number: CN109640941A, publication date: 2019-04-16) provides an odorless and highly stable cosmetic composition, which replaces the silicone acrylate dispersant with a silicone elastomer with an emulsifier, and requires the addition of a sponge to achieve a filling effect. However, this method requires the additional addition of a sponge to achieve a stabilizing effect, and the silicone elastomer itself does not have a significant effect.
[0007] The Chinese invention patent application (publication number: CCN109384925A, publication date: 2019-02-26) provides a natural oil-modified silicone elastomer. Although the compatibility with natural oils is improved, natural oils have many by-products, and their reactions are incomplete and they are easily oxidized to produce negative effects such as corruption and sourness.
[0008] A Chinese invention patent application (publication number: CN101616659A, publication date: 2009-12-30) provides a composition containing an organic silicone elastomer gel, which is mainly cross-linked with an organic hydrogen siloxane of a cyclosiloxane containing at least two Si-H chains to obtain a silicone elastomer with a special structure. However, the raw materials of the Si-H-containing cyclic hydrogen siloxane with a special structure are difficult to obtain and are expensive, which is not conducive to industrialization.
[0009] In summary, existing silicone elastomers have the problems of insufficient compatibility resulting in poor transparency of the formula and difficulty in emulsification resulting in oily products. Although the industry has been trying to solve these problems, there are still problems such as the raw materials are difficult to obtain, the price is high, additional additions are required, it is not conducive to industrialization, and there are many side reactions. Summary of the invention
[0010] The existing technology has the problems of difficult raw materials, difficulty in industrialization, high cost, etc. The present invention aims at the industry problems of insufficient compatibility and difficulty in emulsification, and provides a simple, easy and industrially mass-produced non-oiling silicone elastomer. The silicone elastomer has the characteristics of being non-oiling, good compatibility and easy emulsification.
[0011] In order to achieve the above-mentioned purpose, the present invention adopts the following technical solutions:
[0012] A silicone elastomer, the structural formula of which is as follows:
[0013] ;
[0014] Wherein a=2-50, b=1-1000, c=1-20, d=1-20, e=1-500, f=1-20; c+d=2-40; R1, R2, R3 are saturated silane end-capping groups, and R4 is a hydrophilic polyether group.
[0015] Preferably, a=5-20, b=5-400, c=1-10, d=1-10, e=5-200, f=2-10, c+d=2-20.
[0016] Preferably, R1, R2, and R3 are R2Me3Si, Et3Si, Ph3Si, Pr3Si, and Bu3Si, wherein Me is methyl, Et is ethyl, Ph is phenyl, Pr is isopropyl, and Bu is butyl; preferably, R1 and R2 are Me3Si, Et3Si, and Ph3Si; more preferably, R1, R2, and R3 are the same.
[0017] Preferably, R4 is prepared from terminal unsaturated polyoxyalkylene ether, and the structural formula of terminal unsaturated polyoxyalkylene ether is R5OEO m PO n BO oR6, wherein EO is a polyoxyethylene group, PO is a polyoxypropylene group, and BO is a polyoxybutylene group;
[0018] Wherein m=1-20, n=0-20, o=0-20, preferably, m=1-15, n=0-10, o=0-5;
[0019] Wherein R5 is a monounsaturated olefinic bond, preferably one of vinyl, allyl, methylallyl, ethynyl, propargyl, methylpropargyl, more preferably one of vinyl, allyl and methylallyl;
[0020] R6 is a saturated end-capping group, specifically one of hydroxyl, methyl, ethyl, propyl, methyl isopropyl and acetyl, and more preferably one of hydroxyl, methyl and acetyl.
[0021] Furthermore, the present invention also provides a method for preparing the organosilicon elastomer, wherein the raw materials for preparing the organosilicon elastomer in the method include:
[0022] Component a has a side chain containing hydrogen polysiloxane,
[0023] b component terminal unsaturated polyoxyalkylene ether,
[0024] C component double-terminal unsaturated olefinic polysiloxane,
[0025] Component d: hydrosilylation catalyst,
[0026] and e-component diluent, and is prepared by chemical cross-linking reaction of the raw materials;
[0027] The molar ratio of Si-H units in the a component to the total unsaturated groups in the b component and the c component is (1-1.5): (0.5-1.5), wherein the mass ratio of the b component to the c component is (0.1-0.9): (0.9-0.1); the hydrosilylation catalyst is 1-1000 ppm of the total mass, preferably 1-100 ppm.
[0028] Preferably, component a contains at least 2 Si-H groups in the molecule and at least 2 branched structures, with a molecular weight of 200-1000, preferably 300-800; component b has a molecular weight of 200-1000, preferably 300-800; component c is a double-terminated vinyl polysiloxane with a molecular weight of 1-1000, preferably 2-500; a vinyl mass fraction of 0.1-10%, preferably 2-8% of a vinyl-terminated polysiloxane; component d is a Pt, Rh or Pd catalyst or a complex thereof, preferably a platinum Pt catalyst, specifically one of a Karstedt catalyst or a Speier catalyst, selected from chloroplatinic acid, platinum black and a platinum-organosilicon complex, preferably chloroplatinic acid, a platinum-organosilicon complex; component e has a viscosity of 0.1-1000 mPas, preferably 0.1-500 mPas.
[0029] As a preference, the structure of component a is: R1O (MeHSiO) c+d (Me2SiO) e (R2OHSi) f (Me2SiO)R1, the structural formula is as follows:
[0030] ;
[0031] And / or, component b has the structural formula of R5OEO m PO n BO o R6,
[0032] Wherein, EO is polyoxyethylene, PO is polyoxypropylene, and BO is polyoxybutylene; m=1-20, n=0-20, o=0-20, preferably, m=1-15, n=0-10, o=0-5; R5 is a monounsaturated olefinic bond, preferably one of vinyl, allyl, methylallyl, ethynyl, propargyl, and methylpropargyl, preferably one of vinyl, allyl, and methylallyl; R6 is a saturated end-capping group, preferably one of hydroxyl, methyl, ethyl, propyl, methylisopropyl, and acetyl, preferably one of hydroxyl, methyl, and acetyl;
[0033] And / or, the structure of component c is: CH2=CHSiO(Me2SiO) b (R3OMeSi) a (Me2SiO)SiCH=CH2, the structural formula is as follows:
[0034] ;
[0035] Wherein a=2-50, b=1-1000; R3 is a saturated siloxyl end-capping group, preferably Me3Si, Et3Si, Ph3Si, Pr3Si or Bu3Si; preferably a=2-20, b=1-400; R3 is a saturated siloxyl end-capping group, preferably Me3Si, Et3Si or Ph3Si; Me is methyl, Et is ethyl, Ph is phenyl, Pr is isopropyl, Bu is butyl;
[0036] and / or, component e includes one or more combinations of silicone oil, natural organic oil, and organic solvent;
[0037] The organic silicone oil is at least one of cyclosiloxane, linear polysiloxane and branched polysiloxane, with a viscosity of 0.65-1000; wherein the cyclosiloxane is D4, D5 or D6; the linear polysiloxane is one of methyl silicone oil, ethyl silicone oil, propyl silicone oil and phenyl silicone oil with a viscosity of 0.65-1000 mPas; the branched polysiloxane is one or more of branched methyl silicone oil, branched ethyl silicone oil and branched phenyl silicone oil;
[0038] The natural organic oil is one or more combinations of sunflower oil, corn oil, soybean oil, olive oil, coconut oil, shea butter, squalane, and natural oils;
[0039] The organic solvents are alcohols and hydrocarbon solvents, and the alcohols are specifically one or more combinations of methanol, ethanol, isopropanol, polyethylene glycol, cyclohexanol, propylene glycol, glycerol, etc.; the hydrocarbon solvents are specifically one or more combinations of aromatic hydrocarbons, aliphatic hydrocarbons, fatty ketones, aromatic ketones, aromatic aldehydes, specifically one or more combinations of isododecane, isohexadecane, mineral oil, benzene, toluene, etc.
[0040] Furthermore, the present invention also provides an organosilicon elastomer gel, which is obtained by grinding the organosilicon elastomer into small pieces, then adding a diluent to swell the pieces, and then dispersing the pieces at high speed to obtain the organosilicon elastomer gel.
[0041] Furthermore, the present invention also provides the use of the organosilicon elastomer gel in the preparation of sunscreen, color makeup and skin care cosmetics.
[0042] Furthermore, the present invention also provides a sunscreen gel composition, comprising silicone elastomer gel A, sunscreen agent B, antioxidant C, film former D, and diluent E;
[0043] Silicone elastomer gel A: the silicone elastomer gel according to claim 8;
[0044] Sunscreen B: one or more combinations of physical sunscreens or chemical sunscreens; preferably, the physical sunscreen is one or more combinations of titanium dioxide and zinc dioxide; preferably, the chemical sunscreen is one or more combinations of octyl methoxycinnamate, ethylhexyl methoxycinnamate, octocrylene, avobenzone, oxybenzone, octyl triazone, menthyl anthranilate, 3,4-methylbenzylidene camphor, and bis-ethylhexyloxyphenol methoxyphenyl triazine;
[0045] Antioxidant C: one or more combinations of vitamin E, BHT, and hindered phenols.
[0046] Film former D: one or more combinations of MQ resin and its solution, acrylic resin and its solution, IPDI resin and its solution, MDI and its solution;
[0047] Diluent E: includes one or more combinations of silicone oil, organic oil, and organic solvent; preferably water, cyclosiloxane, linear siloxane, branched siloxane, isomeric alkanes, and alcohols; more preferably water, cyclopentasiloxane, polydimethylsiloxane, octyl polymethylsiloxane, isododecane, and isomeric hexadecane.
[0048] Furthermore, the present invention also provides a method for preparing the sunscreen gel containing the silicone elastomer gel, which is specifically as follows:
[0049] Stir sunscreen B, antioxidant C, film former D and diluent E at a speed of 500-1000 rpm for 30-60 minutes until they are uniform; then add silicone elastomer gel A and stir at a speed of 500-1000 rpm for 1-3 hours until they are in a uniform paste state; finally add diluent E for emulsification and uniform dispersion, and disperse at a speed of 1000-2000 rpm for 1-3 hours until a uniform gel-paste composition is obtained.
[0050] Other ingredients, including but not limited to active ingredients, health ingredients, nutritional ingredients, adsorbents and other ingredients, are determined according to usage requirements.
[0051] The present invention uses the above components as raw materials, performs a silylation and crosslinking reaction under the action of a catalyst, thereby forming an organic silicon elastomer, and performs swelling and dilution under the action of a diluent, thereby forming an organic silicon elastomer gel.
[0052] The Si-H groups in (a) crosslink with the unsaturated olefinic groups in (b) and (c) components to form a network structure. If the ratio is too high, the crosslinking is excessive and the silicone elastomer is too hard, making the particles hard and the skin feel rough; if the ratio is too low, the gel is insufficient, making the product greasy, the skin feel is not refreshing and not silky enough. The appropriate ratio of Si-H and unsaturated groups helps the silicone elastomer gel have a silky, powdery skin feel.
[0053] The present invention uses a Si-H polysiloxane (a) component with a branched structure and a (c) component with an unsaturated alkenyl group with a branched structure to carry out a crosslinking reaction, and introduces a local branched structure to provide a fullness of the silicone elastomer, making the skin feel more silky; at the same time, the branched structure makes the unit molecular structure cavity more and more three-dimensional, providing sufficient cavities for the diluent, making the silicone gel swell more thoroughly and fully, and the final product more stable and oil-free; in addition, the branched structure provides dispersed and dense cavities due to steric hindrance, and can also absorb ingredients such as sunscreen in the cosmetic formula, providing sufficient suspension stability. The local branched structure makes the silicone gel itself more stable and the formula more stable.
[0054] The present invention also endows the silicone elastomer with excellent self-emulsifying properties by introducing hydrophilic groups such as polyoxyalkylene ether, wherein the component (b) is grafted into the cross-linked structure of the silicone elastomer using single-end unsaturated olefinic polyoxyalkylene ether, providing hydrophilicity and self-emulsifying properties while retaining the unique skin feel of the cross-linked body itself. The mode of locking one end and flexibly swinging the other end is adopted, and the flexible swing of the other end provides an opportunity for full contact with water, thereby enhancing the hydrophilicity and emulsifying properties; in addition, the polyether segment provides compatibility with the formula components through the hydrogen bonding of the polyoxyalkylene ether, and the folding and bending properties of the linear structure provide more cavities, which is helpful for the dispersion stability of diluents, powders, macromolecular raw materials, etc.
[0055] The present invention uses physical and chemical reactions of various raw materials, cavities provided by branched structures, and hydrophilic emulsification properties provided by hydrophilic groups such as polyoxyalkylene ethers to make the silicone elastomer gel have excellent skin feel, and the product is less likely to produce oil and is more stable, while also improving the compatibility and stability of cosmetic formulas.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] (1) By increasing the steric hindrance of the network structure inside the silicone elastomer gel, the connecting part is locally branched, thereby increasing the volume of a single silicone elastomer molecule and providing enough gaps and space, which is conducive to swelling and dilution by grease, diluents, etc., avoiding oil leakage.
[0058] (2) By locally introducing the polyoxyalkylene ether structure to provide hydrophilic properties and excellent self-emulsification properties, the use of emulsifiers can be reduced; and since it is connected to the end of the silicone chain on one side, the polyoxyalkylene ether chain has flexibility in the molecule, making it easier for it to fully contact with water to emulsify, and at the same time, as the molecular chain bends, it helps to disperse the powder. It can achieve water absorption, emulsification, and dispersion effects, solving the problem of difficult emulsification of silicone elastomers and improving the physical stability of the formula.
[0059] (3) By adding silicone elastomers to provide a branched structure with steric hindrance and polyoxyethylene ether to increase hydrophilicity, the combined effect helps physical UV blockers enter the gaps to improve the stability of physical sunscreens, while increasing the compatibility of chemical sunscreens, making the formula ingredients more evenly dispersed, thereby improving the stability of the formula.
[0060] (4) By adding a branched structure to provide steric hindrance to the silicone elastomer and a polyoxyalkylene ether to enhance the hydrophilicity, the silicone elastomer can provide moisturizing and water-retaining properties while maintaining the special silky and soft skin feel of the silicone elastomer, and has both a unique skin feel and emulsification function. In addition, the silicone elastomer gel is made more stable and less likely to produce oil, while improving the stability of the application formula composition.
[0061] (5) The raw materials of the silicone elastomer gel of the present invention are easily available, the process is simple, the cost is reasonable, and it is easy to industrialize and produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 This is the infrared spectrum of the silicone elastomer gel prepared in Example 3 of the present invention.
[0063] Figure 2 This is a picture of the silicone elastomer gel prepared in Example 3 of the present invention.
[0064] Figure 3 This is a picture of the self-emulsified silicone elastomer gel prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0065] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0066] Example 1
[0067] Step 1: Preparation of cross-linked silicone elastomer
[0068] Under nitrogen atmosphere, 30% of diluent isododecane was added to the reaction equipment, and then 10 mol of side chain hydrogen-containing polysiloxane with a viscosity of 108 mPas and a hydrogen content of 0.05% (including 10% trimethylsilyl branched structure) was added, and then 2 mol of terminal allyl polyoxyethylene ether (10 EO, OH capped) with a molecular weight of 500 was added to the reactor, and the three raw materials were stirred and mixed at 100 rpm for 0.5 h until uniform, and then 20 ppm of chloroplatinic acid-isopropanol catalyst was added, and the temperature was raised to 60°C for addition reaction for 3 h to obtain a transparent liquid mixture; then 8 mol of double-terminal vinyl polysiloxane with a viscosity of 105 mPas and a vinyl content of 5% (including 10% trimethylsilyl branched structure) was added, and the temperature was continued to be raised to 90°C for cross-linking reaction for 5 h to obtain a silicone cross-linked elastomer.
[0069] Step 2: Preparation of silicone elastomer gel
[0070] The above-mentioned silicone cross-linked elastomer is ground into small pieces, and then 30% of the diluent cyclopentasiloxane is added to swell and dilute it, and then it is dispersed evenly at high speed to obtain a silicone elastomer gel, which has a white foggy paste appearance, a viscosity of 4310 Pas, a solid content of 39.3%, and an oil yield of 0.2% after testing.
[0071] Example 2
[0072] Step 1: Preparation of cross-linked silicone elastomer
[0073] Under nitrogen atmosphere, 30% of diluent isododecane was added to the reaction equipment, and then 10 mol of side chain hydrogen-containing polysiloxane with a viscosity of 20 mPas and a hydrogen content of 0.1% (including 10% triphenylsilyl branched structure) was added, and then 1 mol of terminal methyl allyl polyoxyethylene polyoxypropylene ether (9 EO, 3 PO, methyl end-capped) with a molecular weight of 800 was added to the reactor, and the three raw materials were stirred and mixed at 100 rpm for 0.5 h until uniform, and then 20 ppm of chloroplatinic acid-isopropanol catalyst was added, and the temperature was raised to 60° C. for addition reaction for 3 h to obtain a transparent liquid mixture; then 9 mol of double-terminal vinyl polysiloxane with a viscosity of 480 mPas and a vinyl content of 8% (including 10% triphenylsilyl branched structure) was added, and the temperature was continued to be raised to 90° C. for cross-linking reaction for 5 h to obtain a silicone cross-linked elastomer.
[0074] Step 2: Preparation of silicone elastomer gel
[0075] The above-mentioned silicone cross-linked elastomer is ground into small pieces, and then 40% of the diluent cyclopentasiloxane is added for swelling and dilution, and then dispersed evenly at high speed to obtain a silicone elastomer gel, which has a white foggy paste appearance, a viscosity of 2212 Pas, a solid content of 30.1%, and an oil yield of 0.1% after testing.
[0076] Example 3
[0077] Step 1: Preparation of cross-linked silicone elastomer
[0078] Under nitrogen atmosphere, 30% of diluent cyclopentasiloxane was added to the reaction equipment, and then 10 mol of side chain hydrogen-containing polysiloxane with a viscosity of 280 mPas and a hydrogen content of 0.075% (including 15% triethylsilyl branched structure) was added, and then 2 mol of terminal vinyl polyoxyethylene ether (5 EO, acetyl end-capped) with a molecular weight of 300 was added to the reactor, and the three raw materials were stirred and mixed at 100 rpm for 0.5 h until uniform, and then 10 ppm of chloroplatinic acid-isopropanol catalyst was added, and the temperature was raised to 60°C for addition reaction for 3 h to obtain a transparent liquid mixture; then 7 mol of double-terminal vinyl polysiloxane with a viscosity of 2 mPas and a vinyl content of 3% (including 15% triethylsilyl branched structure) was added, and the temperature was continued to be raised to 90°C for cross-linking reaction for 5 h to obtain a silicone cross-linked elastomer.
[0079] Step 2: Preparation of silicone elastomer gel
[0080] The above-mentioned silicone cross-linked elastomer is ground into small pieces, and then 40% of the diluent cyclopentasiloxane is added to swell and dilute it, and then it is dispersed evenly at high speed to obtain a silicone elastomer gel, which has a white foggy paste appearance, a viscosity of 3235 Pas, a solid content of 28.4%, and an oil yield of 0.5% after testing.
[0081] Example 4 Sunscreen gel composition
[0082] The raw materials of the sunscreen gel composition are shown in Table 1.
[0083] Table 1 Raw materials of sunscreen gel composition
[0084]
[0085] Sunscreen B, antioxidant C, film former D and diluent E were stirred at 800 rpm for 60 min until they were uniform; then silicone elastomer gel A was added and stirred at 1000 rpm for 2 h until they were in a uniform paste state; finally, diluent E was added for emulsification and uniform dispersion, and dispersed at 2000 rpm for 3 h until a uniform gel-paste composition was obtained.
[0086] Comparative Example 1
[0087] Step 1: Preparation of cross-linked silicone elastomer
[0088] Under nitrogen atmosphere, 30% of diluent isododecane was added to the reaction equipment, and then 10 mol of linear side chain hydrogen-containing polysiloxane with a viscosity of 108 mPas and a hydrogen content of 0.05% was added, and then 2 mol of terminal allyl polyoxyethylene ether (10 EO, OH end-capped) with a molecular weight of 500 was added to the reactor, and the three raw materials were stirred and mixed at 100 rpm for 0.5 h until uniform, and then 20 ppm of chloroplatinic acid-isopropanol catalyst was added, and the temperature was raised to 60°C for addition reaction for 3 h to obtain a transparent liquid mixture; then 8 mol of double-terminal vinyl polysiloxane with a viscosity of 105 mPas and a vinyl content of 5% (including 10% trimethylsilyl branched structure) was added, and the temperature was continued to be raised to 90°C for cross-linking reaction for 5 h to obtain a silicone cross-linked elastomer.
[0089] Step 2: Preparation of silicone elastomer gel
[0090] The above-mentioned silicone cross-linked elastomer is ground into small pieces, and then 30% of the diluent cyclopentasiloxane is added for swelling and dilution, and then dispersed evenly at high speed to obtain a silicone elastomer gel, which has a white foggy paste appearance, a viscosity of 3878 Pas, a solid content of 39.8%, and an oil yield of 5.1% after testing.
[0091] Comparative Example 2
[0092] Step 1: Preparation of cross-linked silicone elastomer
[0093] Under nitrogen atmosphere, 30% of diluent isododecane was added to the reaction equipment, and then 10 mol of side chain hydrogen-containing polysiloxane with a viscosity of 108 mPas and a hydrogen content of 0.05% (including 10% trimethylsilyl branched structure) was added, and then 2 mol of terminal allyl polyoxyethylene ether (10 EO, OH capped) with a molecular weight of 500 was added to the reactor, and the three raw materials were stirred and mixed at 100 rpm for 0.5 h until uniform, and then 20 ppm of chloroplatinic acid-isopropanol catalyst was added, and the temperature was raised to 60°C for addition reaction for 3 h to obtain a transparent liquid mixture; then 8 mol of bilinear terminal vinyl polysiloxane with a viscosity of 105 mPas and a vinyl content of 5% was added, and the temperature was continued to be raised to 90°C for cross-linking reaction for 5 h to obtain a silicone cross-linked elastomer.
[0094] Step 2: Preparation of silicone elastomer gel
[0095] The above-mentioned silicone cross-linked elastomer is ground into small pieces, and then 30% of the diluent cyclopentasiloxane is added for swelling and dilution, and then dispersed evenly at high speed to obtain a silicone elastomer gel, which has a white foggy paste appearance, a viscosity of 4121 Pas, a solid content of 38.4%, and an oil yield of 3.0% after testing.
[0096] Comparative Example 3
[0097] Step 1: Preparation of cross-linked silicone elastomer
[0098] Under a nitrogen atmosphere, 30% of the diluent isododecane was added to the reaction equipment, and then 10 mol of a linear side-chain hydrogen-containing polysiloxane with a viscosity of 108 mPas and a hydrogen content of 0.05% was added, and then 2 mol of terminal allyl polyoxyethylene ether (10 EO, OH capped) with a molecular weight of 500 was added to the reactor. The three raw materials were stirred and mixed at 100 rpm for 0.5 h until uniform, and then 20 ppm of chloroplatinic acid-isopropanol catalyst was added, and the temperature was raised to 60°C for addition reaction for 3 h to obtain a transparent liquid mixture; then 8 mol of a linear double-terminal vinyl polysiloxane with a viscosity of 105 mPas and a vinyl content of 5% was added, and the temperature was continued to be raised to 90°C for cross-linking reaction for 5 h to obtain a silicone cross-linked elastomer.
[0099] Step 2: Preparation of silicone elastomer gel
[0100] The above-mentioned silicone cross-linked elastomer is ground into small pieces, and then 30% of the diluent cyclopentasiloxane is added to swell and dilute it, and then it is dispersed evenly at high speed to obtain a silicone elastomer gel, which has a white foggy paste appearance, a viscosity of 3512 Pas, a solid content of 38.9%, and an oil yield of 10.8% after testing.
[0101] Table 2 Differences between the raw materials and product performance of the embodiments and comparative examples
[0102]
[0103] The above is a description of the embodiments of the present invention. Through the above description of the disclosed embodiments, professionals and technicians in the field can implement or use the present invention. Various modifications to these embodiments will be apparent to professionals and technicians in the field. The general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown in this article, but will conform to the widest range consistent with the principles and novelties disclosed herein.
Claims
1. A silicone elastomer, the structural formula of which is as follows: ; Wherein a=2-50, b=1-1000, c=1-20, d=1-20, e=1-500, f=1-20; R1, R2, R3 are saturated silane end-capping groups, R4 is prepared from terminal unsaturated polyoxyalkylene ether, and the structural formula of the terminal unsaturated polyoxyalkylene ether is R5OEO m PO n BO o R6, wherein EO is a polyoxyethylene group, PO is a polyoxypropylene group, and BO is a polyoxybutylene group; Where m=1-20, n=0-20, o=0-20; Wherein R5 is a monounsaturated olefinic bond, and R6 is a saturated end-capping group.
2. The organic silicone elastomer according to claim 1, characterized in that: a=5-20, b=5-400, c=1-10, d=1-10, e=5-200, f=2-10, c+d=2-20.
3. The organic silicone elastomer according to claim 1, characterized in that: R1, R2, and R3 are Me3Si, Et3Si, Ph3Si, Pr3Si, or Bu3Si, Me is a methyl group, Et is an ethyl group, Ph is a phenyl group, Pr is an isopropyl group, and Bu is a butyl group.
4. The organic silicone elastomer according to claim 3, characterized in that: R1 and R2 are Me3Si, Et3Si or Ph3Si.
5. The organic silicone elastomer according to claim 1, characterized in that: m=1-15, n=0-10, o=0-5; and / or, R5 is one of vinyl, allyl, methylallyl, ethynyl, propargyl, and methylpropargyl; And / or, R6 is one of hydroxyl, methyl, ethyl, propyl, methyl isopropyl and acetyl.
6. The organic silicone elastomer according to claim 1, characterized in that: R5 is one of vinyl, allyl and methallyl; and / or R6 is one of hydroxyl, methyl and acetyl.
7. The method for preparing the silicone elastomer according to any one of claims 1 to 6, characterized in that: The raw materials for preparing the organic silicon elastomer in the method include: Component a has a side chain containing hydrogen polysiloxane, b component terminal unsaturated polyoxyalkylene ether, C component double-terminal unsaturated olefinic polysiloxane, Component d: hydrosilylation catalyst, and e-component diluent, and is prepared by chemical cross-linking reaction of the raw materials; The molar ratio of Si-H units in the a component to the total unsaturated groups in the b component and the c component is (1-1.5): (0.5-1.5), wherein the mass ratio of the b component to the c component is (0.1-0.9): (0.9-0.1).
8. The preparation method according to claim 7, characterized in that: The hydrosilylation catalyst is 1-1000 ppm of the total mass.
9. The preparation method according to claim 7, characterized in that: The hydrosilylation catalyst is 1-100 ppm of the total mass.
10. The preparation method according to claim 7, characterized in that: The a component has at least two Si-H groups in the molecule and at least two branched structures, with a molecular weight of 200-1000; the b component has a molecular weight of 200-1000; the c component is a double-terminal vinyl polysiloxane, with a molecular weight of 1-1000 and a vinyl mass fraction of 0.1-10%; the d component is a Pt, Rh or Pd catalyst or its complex; The viscosity of component e is 0.1-1000 mPas.
11. The preparation method according to claim 7, characterized in that: The molecular weight of component a is 300-800; the molecular weight of component b is 300-800; the molecular weight of component c is 2-500; and / or, component c is 2-8% of vinyl terminated polysiloxane; and / or, component d is one of a Karstedt catalyst or a Speier catalyst; And / or, the viscosity of component e is 0.1-500 mPas.
12. The preparation method according to claim 7, characterized in that: a component structure: R1O (MeHSiO) c+d (Me2SiO) e (R2OHSi) f (Me2SiO)R1, the structural formula is as follows: ; And / or, component b has the structural formula of R5OEO m PO n BO o R6, Wherein, EO is polyoxyethylene, PO is polyoxypropylene, BO is polyoxybutylene; m=1-20, n=0-20, o=0-20; And / or, the structure of component c is: CH2=CHSiO(Me2SiO) b (R3OMeSi) a (Me2SiO)SiCH=CH2, the structural formula is as follows: ; And / or, component e includes one or more combinations of silicone oil, natural organic oil, and organic solvent.
13. The preparation method according to claim 12, characterized in that: The organic silicone oil is at least one of cyclosiloxane, linear polysiloxane and branched polysiloxane, with a viscosity of 0.65-1000; wherein the cyclosiloxane is D4, D5 or D6; the linear polysiloxane is one of methyl silicone oil, ethyl silicone oil, propyl silicone oil and phenyl silicone oil with a viscosity of 0.65-1000 mPas; the branched polysiloxane is one or more of branched methyl silicone oil, branched ethyl silicone oil and branched phenyl silicone oil; And / or, the natural organic oil is one or more combinations of sunflower oil, corn oil, soybean oil, olive oil, coconut oil, shea butter, and squalane; And / or, the organic solvent is an alcohol or hydrocarbon solvent, the alcohol is specifically one or more combinations of methanol, ethanol, isopropanol, polyethylene glycol, cyclohexanol, propylene glycol, glycerol, etc.; the hydrocarbon solvent is specifically one or more combinations of aromatic hydrocarbons and aliphatic hydrocarbons.
14. A silicone elastomer gel, characterized in that: The silicone elastomer gel can be obtained by grinding the silicone elastomer described in any one of claims 1 to 6 into small pieces, then adding a diluent to swell it, and then dispersing it evenly at high speed.
15. Use of the organosilicon elastomer gel according to claim 14 in the preparation of skin care cosmetics.
16. Use of the organosilicon elastomer gel according to claim 14 in the preparation of sunscreen or color cosmetics.
17. A skin care cosmetic comprising the silicone elastomer gel according to claim 14.
18. A sunscreen or makeup product, comprising the organosilicon elastomer gel according to claim 14.
19. A sunscreen gel composition, comprising silicone elastomer gel A, sunscreen agent B, antioxidant C, film former D, and diluent E; Silicone elastomer gel A: the silicone elastomer gel according to claim 14; Sunscreen B: one or more combinations of physical sunscreens or chemical sunscreens; Antioxidant C: one or more combinations of vitamin E and hindered phenols; Film former D: one or more combinations of MQ resin and its solution, acrylic resin and its solution, IPDI resin and its solution, MDI and its solution; Diluent E: includes one or more combinations of silicone oil, organic oil and organic solvent.
20. A sunscreen gel composition according to claim 19, characterized in that: Antioxidant C is BHT.
21. A sunscreen gel composition according to claim 19, characterized in that: Physical sunscreens are one or more combinations of titanium dioxide and zinc dioxide; chemical sunscreens are one or more combinations of octyl methoxycinnamate, ethylhexyl methoxycinnamate, octocrylene, avobenzone, oxybenzone, octyl triazone, menthyl anthranilate, 3,4-methylbenzylidene camphor, and bis-ethylhexyloxyphenol methoxyphenyl triazine; And / or, the diluent E is water, cyclosiloxane, linear siloxane, branched siloxane, isomeric alkane, alcohol.
Citation Information
Patent Citations
Personal care compositions containing silicone elastomer gels
CN101616659A
Copolymer having carbosiloxane dendrimer structure and composition and cosmetic containing the same
CN104661645A
Natural oil-modified organosilicon elastomer
CN109384925A
Odorless and highly stable cosmetic composition
CN109640941A
Polyfunctional-group-modified polysiloxane emulsifier and preparation method thereof
CN104177620A