A high-sensitivity flexible pressure sensor and preparation method thereof

Through the flexible cavity processing technology of graphene/polyimide composite film and copper sacrificial layer, the problem of insufficient sensitivity of existing pressure sensors is solved, and the precise detection of pressure in natural gas wellheads and conveying pipelines is achieved, which improves the sensitivity of the sensor and production efficiency reduces costs.

CN118670596BActive Publication Date: 2024-11-12LIAONING YIDA PETROLEUM ENG CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411148262.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Due to the lack of material characteristics and sensitivity of existing rigid piezoresistive pressure sensors, they cannot meet the pressure detection needs during natural gas mining and transportation, and can easily lead to blowouts and pipeline safety accidents.

Method used

A graphene/polyimide composite film is used as a pressure-sensitive unit, and a flexible cavity processing technology of copper sacrificial layer and release holes is combined with a flexible cavity processing technology. Water transfer and reactive ion etching technology are used to prepare a flexible pressure sensor with high sensitivity.

Benefits of technology

It realizes accurate detection of pressure changes in natural gas wellheads and conveying pipelines, improves sensor sensitivity and production efficiency, reduces costs, is compatible with MEMS processes, and is suitable for large-scale manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118670596B_ABST
    Figure CN118670596B_ABST
Patent Text Reader

Abstract

The present invention relates to a highly sensitive flexible pressure sensor and a preparation method thereof, wherein the pressure sensor comprises: a substrate; a cavity located in the middle of the substrate; a pressure sensitive unit located above the cavity; a detection electrode arranged on the upper surface of the substrate, and the detection electrode is partially covered by the pressure sensitive unit. The pressure sensitive unit is a graphene / polyimide composite film. The sensor uses a graphene film grown by CVD as a pressure sensitive layer, has extremely high sensitivity, and can accurately detect pressure changes at the wellhead of a natural gas extraction well or in a natural gas transmission pipeline.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of pressure sensors, and in particular to a high-sensitivity flexible pressure sensor and a preparation method thereof. Background Art

[0002] Pressure sensors have broad application prospects in the fields of automotive electronics, biomedicine, aerospace, and natural gas. Rigid piezoresistive pressure sensor is a device that uses the piezoresistive properties of doped silicon to detect pressure.

[0003] During the natural gas extraction process, if the pressure in the extraction well is too high, blowouts are likely to occur. For the safe production of natural gas, a highly sensitive pressure sensor is needed to detect pressure changes at the wellhead of the extraction well in order to prevent blowouts.

[0004] Moreover, in the process of natural gas transportation, pressure is one of the key indicators. Reasonable gas pressure can ensure the fluidity of natural gas in the pipeline and enable it to reach users smoothly. However, too high or too low gas pressure may cause pipeline rupture, leakage and other safety accidents. It is very necessary to accurately detect natural gas pressure.

[0005] The rigid piezoresistive pressure sensor is limited by its own material properties of small piezoresistance coefficient and high device stiffness, and its sensitivity can no longer meet the needs.

[0006] Therefore, there is an urgent need for a flexible pressure sensor with high sensitivity. Summary of the invention

[0007] In order to solve at least part of the above problems in the prior art, the present invention provides a high-sensitivity flexible pressure sensor, comprising:

[0008] substrate;

[0009] a cavity located in the middle of the substrate;

[0010] a pressure sensitive unit located above the cavity;

[0011] The detection electrode is arranged on the upper surface of the substrate, and a portion of the detection electrode is covered by the pressure sensitive unit.

[0012] Furthermore, the pressure sensitive unit is a graphene / polyimide composite film.

[0013] Furthermore, the detection electrode comprises:

[0014] Electrode pads;

[0015] A plurality of leads are connected to the electrode pads, wherein a portion of the plurality of leads is covered by the sensitive unit.

[0016] Furthermore, the substrate comprises:

[0017] a first polyimide film;

[0018] The second polyimide film is located on the first polyimide film.

[0019] Furthermore, the depth of the cavity is located in the second polyimide film, and the depth of the cavity is less than the thickness of the second polyimide film.

[0020] Further, the thickness of the pressure sensitive unit is 0.5 μm-2 μm; and / or

[0021] The size of the electrode pad is , the lead size is , with a thickness of 100nm-200nm; and / or

[0022] The thickness of the second polyimide film retained above the cavity is 1 μm-3 μm; and / or

[0023] The thickness of the first polyimide film and / or the second polyimide film is 10 μm-20 μm.

[0024] The present invention also provides a method for preparing a high-sensitivity flexible pressure sensor, comprising:

[0025] forming a first polyimide film on the surface of the carrier;

[0026] forming a metal seed layer on the first polyimide film;

[0027] Arranging photoresist on the seed layer and performing photolithography development to obtain a sacrificial layer pattern;

[0028] forming a metal sacrificial layer in the sacrificial layer pattern, and then removing the photoresist;

[0029] forming a second polyimide film on the metal seed layer and the metal sacrificial layer;

[0030] Arranging a photoresist on the second polyimide film and performing photolithography development to obtain an electrode pattern;

[0031] Arranging metal in the electrode pattern to obtain a patterned detection electrode, and then removing the photoresist;

[0032] Arranging photoresist on the second polyimide film and performing photolithography and development to form a hole pattern above the metal sacrificial layer, while removing the photoresist located at the periphery of the detection electrode;

[0033] The exposed second polyimide film is etched to obtain a release hole, and the second polyimide film located at the periphery of the detection electrode is removed to expose the metal seed layer, and then the photoresist is removed;

[0034] soaking the metal sacrificial layer below the release hole in a metal etching solution to obtain a cavity, and etching the exposed metal seed layer to expose the first polyimide film; and

[0035] The graphene / polyimide composite film is transferred onto the second polyimide film and the first polyimide film by water transfer printing.

[0036] Furthermore, it also includes:

[0037] Arranging a photoresist on the graphene / polyimide composite film, performing photolithography development, and obtaining an etching mask of the graphene / polyimide composite film;

[0038] Etching the exposed graphene / polyimide film to obtain a patterned graphene / polyimide composite film, and then removing the photoresist, wherein the patterned graphene / polyimide composite film is located above the cavity and covers a portion of the detection electrode; and

[0039] Connect the wires to the detection electrodes by welding.

[0040] Furthermore, the method of transferring the graphene / polyimide composite film to the second polyimide film and the first polyimide film by water transfer printing comprises:

[0041] Growing graphene on copper foil, forming a layer of polyimide on the graphene, and obtaining a graphene / polyimide composite film, wherein the composite film structure is copper foil-graphene-polyimide;

[0042] The copper foil with the graphene / polyimide composite film is transferred into a copper etching solution to release the copper foil, thereby obtaining the graphene-polyimide composite film;

[0043] The graphene / polyimide composite film is transferred to deionized water and allowed to stand, and the graphene / polyimide composite film is automatically flattened;

[0044] The composite membrane was scooped up in deionized water using the support with the cavity prepared, and then annealed.

[0045] Furthermore, the detection electrode comprises:

[0046] Electrode pads;

[0047] A plurality of leads are connected to the electrode pads, wherein a portion of the plurality of leads is covered by the graphene / polyimide film.

[0048] The present invention has at least the following beneficial effects: (1) The sensor uses a graphene film grown by CVD as a pressure sensitive layer, which has extremely high sensitivity and can accurately detect pressure changes at the wellhead of a natural gas production well or in a natural gas transmission pipeline. (2) In the preparation process of the pressure sensor of the present invention, a flexible cavity processing technology based on a copper sacrificial layer and a release hole is used. Compared with the traditional method of using lasers for local hole opening, this method can be compatible with MEMS process wafer-level processing, parallel manufacturing, and low cost; (3) The graphene / polyimide composite film grown by water transfer CVD is used and patterned by reactive ion etching, which ensures that the thickness of the graphene film is thin enough while having the processing method of large-scale patterned graphene, thereby ensuring the sensitivity and production yield of the sensor. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to further illustrate the above and other advantages and features of various embodiments of the present invention, a more specific description of various embodiments of the present invention will be presented with reference to the accompanying drawings. It will be understood that these drawings only depict typical embodiments of the present invention and are therefore not to be considered as limiting the scope thereof. In the accompanying drawings, for clarity, identical or corresponding parts will be represented by identical or similar reference numerals.

[0050] Figure 1 A perspective view of a high-sensitivity flexible pressure sensor according to an embodiment of the present invention is shown;

[0051] Figure 2 A top view of a highly sensitive flexible pressure sensor according to an embodiment of the present invention is shown;

[0052] Figure 3 A side view of a highly sensitive flexible pressure sensor according to an embodiment of the present invention is shown; and

[0053] Figure 4 A process flow chart for preparing a high-sensitivity flexible pressure sensor according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0054] It should be noted that various components in the various drawings may be shown exaggeratedly for illustrative purposes and are not necessarily correct to scale.

[0055] In the present invention, each embodiment is only intended to illustrate the aspects of the present invention and should not be construed as limiting.

[0056] In the present invention, unless otherwise specified, the quantifiers "a", "an" and "an" do not exclude the presence of a plurality of elements.

[0057] It should also be pointed out that in the embodiments of the present invention, for the sake of clarity and simplicity, only a portion of the parts or components may be shown, but a person of ordinary skill in the art will understand that under the teachings of the present invention, required parts or components may be added as needed in specific scenarios.

[0058] It should also be pointed out that within the scope of the present invention, the terms "same", "equal", "equal to" and the like do not mean that the two values ​​are absolutely equal, but allow a certain reasonable error, that is, the terms also cover "substantially the same", "substantially equal", and "substantially equal to".

[0059] It should also be pointed out that in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than explicitly or implicitly indicating that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as explicitly or implicitly indicating relative importance.

[0060] In addition, the embodiments of the present invention describe the process steps in a specific order, but this is only for the convenience of distinguishing the steps, and does not limit the sequence of the steps. In different embodiments of the present invention, the sequence of the steps can be adjusted according to the adjustment of the process.

[0061] Figure 1 A perspective view of a high-sensitivity flexible pressure sensor according to an embodiment of the present invention is shown; Figure 2 A top view of a highly sensitive flexible pressure sensor according to an embodiment of the present invention is shown; Figure 3 A side view of a highly sensitive flexible pressure sensor according to an embodiment of the present invention is shown.

[0062] like Figures 1 to 3 As shown, a high-sensitivity flexible pressure sensor is mainly composed of a substrate 1, a pressure sensitive unit 2, a cavity 3, a detection electrode 4 and a release hole 5.

[0063] The substrate 1 includes a first polyimide film 11 and a second polyimide film 12 , wherein the second polyimide film 12 is located on the first polyimide film 11 .

[0064] The first polyimide film 11 provides support for the entire device. In one embodiment of the present invention, the thickness of the first polyimide film 11 is 10 μm-20 μm. In one embodiment of the present invention, the thickness of the second polyimide film 12 is 10 μm-20 μm, and the top view is a square with a side length of 300 μm-500 μm. The first polyimide film 11 and the second polyimide film 12 are the same size.

[0065] The cavity 3 is located in the second polyimide film 12. In one embodiment of the present invention, the cavity 3 is square in top view with a side length of 200 μm-300 μm (smaller than the second polyimide film), and the thickness of the second polyimide film retained above the cavity is 1 μm-3 μm, which is the same as the depth of the release hole.

[0066] The detection electrode 4 is located on the upper surface of the second polyimide film 12 . The detection electrode 4 includes an electrode pad 41 and a plurality of leads 42 . The electrode pad 41 and the leads 42 are connected, and a portion of the plurality of leads 42 is covered by the sensitive unit 2 .

[0067] In one embodiment of the present invention, the electrode pad size is , the lead size is The overall thickness of the electrode is 100nm-200nm, which is used to provide electrical leads. The detection electrode 4 is a Ti / Au electrode, which is divided into two layers, Ti in the lower layer and Au in the upper layer, where Ti is only a thin layer of adhesion to improve the bonding strength, and electrical interconnection mainly relies on Au.

[0068] The detection electrode 4 adopts a multi-finger electrode structure, which can provide multiple conductive paths for graphene to reduce resistance.

[0069] The pressure sensitive unit 2 is arranged on the cavity 3. The pressure sensitive unit 2 is a graphene / polyimide composite film with a thickness of 0.5 μm-2 μm, a square shape in top view, and a side length of 300 μm-400 μm. The film covers the Au lead wire for forming electrical interconnection.

[0070] The release hole 5 is located above the cavity 3, with a diameter of 10μm-20μm and a spacing of 10μm-20μm. The release hole 5 is used to allow the copper etching liquid to enter the lower part to release the Cu sacrificial layer and form a cavity during the release process. For details, see the preparation process below.

[0071] The pressure sensor further includes a wire electrically connected to the electrode pad.

[0072] The working principle of its highly sensitive flexible graphene film pressure sensor is as follows:

[0073] The principle of the above-mentioned flexible pressure sensor is based on the piezoresistive effect. When the graphene / polyimide composite film is in an environment where there is a pressure difference between the upper and lower pressures of the composite film, the surface of the composite film is strained, thereby causing the energy band structure of the graphene to change, changing the carrier mobility of the graphene, and causing resistance changes. The corresponding resistance change is led out through the gold lead, thereby converting the pressure signal into an electrical signal. Compared with the traditional single-crystal silicon piezoresistive sensor, the sensitivity per unit area of ​​the graphene pressure sensor is more than 50 times that of the traditional single-crystal silicon piezoresistive sensor.

[0074] Figure 4 A process flow chart for preparing a high-sensitivity flexible pressure sensor according to an embodiment of the present invention is shown.

[0075] like Figure 4 As shown, the preparation process of the high-sensitivity flexible pressure sensor is as follows:

[0076] Step 1, such as Figure 4 (a) Use 3% HCl solution and 5% NaOH solution and ultrasonic cleaning to remove oil and other pollutants on the surface of the carrier 21, and finally use acetone ultrasonic cleaning and place in a 60 degree Celsius oven to dry. The carrier 21 can be a hard plate such as a glass sheet.

[0077] Step 2, such as Figure 4 (b) Spin-coating a polyimide solution on the surface of the carrier by spin coating, and placing the spin-coated carrier in an oven at 300 degrees Celsius for curing to form a first polyimide film 11 with a thickness of 10 μm to 20 μm.

[0078] Step 3, such as Figure 4 (c) Using a sputtering process, a metal seed layer 23 with a thickness of 200 nm to 300 nm is prepared on the first polyimide film 11. The metal seed layer 23 may be a chromium / copper seed layer.

[0079] Step 4, such as Figure 4 (d) Spin-coat a positive photoresist with a thickness of 10 μm-19 μm on the metal seed layer 23, pre-bake for 60 minutes at 100 degrees Celsius on a hot plate to cure the photoresist, and perform photolithography development using a stepper lithography machine to obtain a sacrificial layer pattern.

[0080] Step 5, such as Figure 4 (e) Electrochemical deposition is performed using a metal plating solution to form a metal sacrificial layer 24 of 10 μm to 19 μm in the area without photoresist (in the sacrificial layer pattern), and the photoresist is removed using acetone. The area of ​​the metal sacrificial layer 24 is smaller than the metal seed layer 23. The metal sacrificial layer 24 can be a copper sacrificial layer.

[0081] Step 6, such as Figure 4(f) Spin-coating the polyimide solution on the metal seed layer 23 and the metal sacrificial layer 24 by a spin coating method, and then curing them in an oven at 300 degrees Celsius to form a second polyimide film 12 with a thickness of 10 μm-20 μm.

[0082] Step 7, such as Figure 4 (g) Spin-coat a positive photoresist with a thickness of 2 μm-5 μm on the second polyimide film 12 by spin coating, pre-bake for 5 minutes at 100 degrees Celsius using a hot plate to solidify the photoresist, and perform photolithography development using a stepper lithography machine to obtain an electrode pattern.

[0083] Step 8, such as Figure 4 (h), using a sputtering process to sputter metal in the electrode pattern to obtain a detection electrode 4 with a thickness of 100nm-200nm, and then using acetone glass photoresist to obtain a patterned detection electrode 4. The detection electrode 4 includes an electrode pad and a plurality of leads. The detection electrode is a titanium / gold electrode layer, in which titanium is located in the lower layer and gold is located in the upper layer, and electrical interconnection is mainly achieved by gold. The detection electrode 4 is a multi-finger electrode, which can provide multiple conductive paths for graphene to reduce resistance.

[0084] Step 9, such as Figure 4 (i) Spin-coat a positive photoresist with a thickness of 10 μm to 19 μm on the second polyimide film, pre-bake the photoresist at 100 degrees Celsius for 60 minutes on a hot plate to solidify the photoresist, and perform photolithography development using a stepper lithography machine to form a hole pattern above the metal sacrificial layer 24. At the same time, remove the photoresist located at the periphery of the detection electrode.

[0085] Step 10, such as Figure 4 (j) The exposed second polyimide film is dry-etched by a reactive ion etcher to obtain a release hole 5, and the second polyimide film located at the periphery of the detection electrode is removed to expose a portion of the metal seed layer, and then the photoresist is removed by acetone.

[0086] Step 11, such as Figure 4 (j) Soak the device in a metal etching solution for 20 minutes to release the metal sacrificial layer 24 below the release hole 5 to obtain a cavity 3. Etch the seed layer exposed by removing the second polyimide film to expose the first polyimide film 11. The thickness of the second polyimide film retained above the cavity is 1μm-3μm. The function of the release hole 5 is to allow the metal etching solution to form contact with the metal sacrificial layer 24 below through the release hole 5, and release the metal sacrificial layer below, thereby forming a cavity, and the thickness of the cavity is less than the thickness of the second polyimide film. The metal etching solution is, for example, a copper etching solution, which removes the copper sacrificial layer. The seed layer etching solution is an etching solution for chromium / copper.

[0087] Step 12, such as Figure 4 (k) The graphene / polyimide composite film 29 is transferred onto the second polyimide film 12 and the exposed first polyimide film 11 by water transfer, wherein the thickness of the graphene / polyimide composite film is 0.5 μm-2 μm. The graphene / polyimide composite film covers the second polyimide film, the first polyimide film and the detection electrode.

[0088] The specific steps of water transfer are as follows: Graphene is grown on copper foil by chemical vapor deposition (CVD) method, and a layer of polyimide is formed on the graphene by spin coating and curing to obtain a graphene / polyimide composite film, and the composite film structure is also: copper foil-graphene-polyimide. The copper foil with the composite film is transferred to the copper etching solution, and the copper foil is released to obtain a graphene-polyimide composite film. The composite film is transferred to deionized water using a glass slide and allowed to stand for one hour. Due to surface tension, the film is automatically flattened. The composite film is picked up in deionized water using a carrier containing polyimide film corresponding to the above process, and annealed in an oven at 150 degrees Celsius for two hours, so that the transfer is successful.

[0089] Step 13, such as Figure 4 (l) Spin-coat a positive photoresist on the graphene / polyimide composite film using a spin coating method, with a thickness of 2 μm-5 μm, and pre-bake the photoresist for 5 minutes at 100 degrees Celsius using a hot plate to cure the photoresist. Perform photolithography development using a stepper lithography machine to obtain an etching mask for the graphene / polyimide composite film.

[0090] Step 14: Figure 4 (m), the exposed graphene / polyimide film is dry-etched by a reactive ion etcher to obtain a patterned graphene / polyimide composite film 29. Finally, the photoresist is removed by acetone. The patterned graphene / polyimide composite film 29 is located above the cavity and covers a portion of the detection electrode.

[0091] Through the above steps, multiple pressure sensors can be manufactured on the carrier at the same time.

[0092] Step 15: Cut the prepared carrier with the pressure sensor into individual sensors along the edge of the second polyimide film.

[0093] Step 16, welding the wire to the detection electrode 4 to ensure electrical conduction, thereby converting the sensitive signal into an electrical signal for export. For example, enameled wire or copper wire is used to weld the detection electrode

[0094] Step 17, remove the carrier.

[0095] The present invention adopts MEMS processing technology to manufacture flexible pressure sensors, which has the advantages of low cost and simple processing method. The present invention proposes a flexible cavity processing technology based on a copper sacrificial layer and a release hole array. Compared with the traditional method of using laser for local hole opening, this method can be compatible with MEMS process wafer-level processing, parallel manufacturing, and low cost.

[0096] The integrated pit manufactured by the non-bonding process simplifies the process flow. The integrated pit manufactured by the non-bonding process means that the traditional silicon piezoresistive pressure sensor uses a cavity to etch the back of the silicon and uses a bonding process to bond a glass sheet to complete the processing, while the preparation process of the present invention does not require a bonding process.

[0097] The graphene / polyimide composite film grown by water transfer CVD and patterned by reactive ion etching ensures that the thickness of the graphene film is thin enough while also having the processing method of large-scale patterned graphene, ensuring the sensitivity and production yield of the sensor.

[0098] Although some embodiments of the present invention have been described in this application document, it will be appreciated by those skilled in the art that these embodiments are merely shown as examples. Those skilled in the art may conceive of numerous variations, alternatives, and improvements under the teachings of the present invention without departing from the scope of the present invention. The appended claims are intended to define the scope of the present invention and to cover methods and structures within the scope of these claims themselves and their equivalents.

Claims

1. A high-sensitivity flexible pressure sensor, characterized in that: include: A substrate, comprising: a first polyimide film; and a second polyimide film, which is located on the first polyimide film; a cavity, which is located in the middle of the substrate, and the cavity is located in the second polyimide film; a release hole, which is located in the second polyimide film and above the cavity, and the thickness of the second polyimide film retained above the cavity is equal to the depth of the release hole; A pressure sensitive unit, which is located above the cavity, and the pressure sensitive unit is a graphene / polyimide composite film; The detection electrode is arranged on the upper surface of the substrate, and a part of the detection electrode is covered by the pressure sensitive unit.

2. The high-sensitivity flexible pressure sensor according to claim 1, characterized in that: The detection electrode comprises: Electrode pads; A plurality of leads are connected to the electrode pads, wherein a portion of the plurality of leads is covered by the sensitive unit.

3. The high-sensitivity flexible pressure sensor according to claim 1, characterized in that: The thickness of the pressure sensitive unit is 0.5 μm-2 μm; and / or The size of the electrode pad is , the lead size is , with a thickness of 100nm-200nm; and / or The thickness of the second polyimide film retained above the cavity is 1 μm-3 μm; and / or The thickness of the first polyimide film and / or the second polyimide film is 10 μm-20 μm.

4. A method for preparing a high-sensitivity flexible pressure sensor, characterized in that: include: forming a first polyimide film on the surface of the carrier; forming a metal seed layer on the first polyimide film; Arranging photoresist on the seed layer and performing photolithography development to obtain a sacrificial layer pattern; forming a metal sacrificial layer in the sacrificial layer pattern, and then removing the photoresist; forming a second polyimide film on the metal seed layer and the metal sacrificial layer; Arranging a photoresist on the second polyimide film and performing photolithography development to obtain an electrode pattern; Arranging metal in the electrode pattern to obtain a patterned detection electrode, and then removing the photoresist; Arranging photoresist on the second polyimide film and performing photolithography and development to form a hole pattern above the metal sacrificial layer, while removing the photoresist located at the periphery of the detection electrode; The exposed second polyimide film is etched to obtain a release hole, and the second polyimide film located at the periphery of the detection electrode is removed to expose the metal seed layer, and then the photoresist is removed; The metal sacrificial layer below the release hole is etched by soaking in a metal etching solution to obtain a cavity, and the exposed metal seed layer is etched to expose the first polyimide film; as well as The graphene / polyimide composite film is transferred onto the second polyimide film and the first polyimide film by water transfer printing.

5. The method for preparing a high-sensitivity flexible pressure sensor according to claim 4, characterized in that: After transferring the graphene / polyimide composite film onto the second polyimide film and the first polyimide film by water transfer printing, the method further includes: Arranging a photoresist on the graphene / polyimide composite film, performing photolithography development, and obtaining an etching mask of the graphene / polyimide composite film; Etching the exposed graphene / polyimide film to obtain a patterned graphene / polyimide composite film, and then removing the photoresist, wherein the patterned graphene / polyimide composite film is located above the cavity and covers a portion of the detection electrode; and Connect the wires to the detection electrodes by welding.

6. The method for preparing a high-sensitivity flexible pressure sensor according to claim 4, characterized in that: The method of transferring the graphene / polyimide composite film to the second polyimide film and the first polyimide film by water transfer printing comprises: Growing graphene on copper foil, forming a layer of polyimide on the graphene, and obtaining a graphene / polyimide composite film, wherein the composite film structure is copper foil-graphene-polyimide; The copper foil with the graphene / polyimide composite film is transferred into a copper etching solution to release the copper foil, thereby obtaining the graphene-polyimide composite film; The graphene / polyimide composite film is transferred to deionized water and allowed to stand, and the graphene / polyimide composite film is automatically flattened; The composite membrane was scooped up in deionized water using the support with the cavity prepared, and then annealed.

7. The method for preparing a high-sensitivity flexible pressure sensor according to claim 5, characterized in that: The detection electrode comprises: electrode pads; and A plurality of leads are connected to the electrode pads, wherein a portion of the plurality of leads is covered by the graphene / polyimide film.

Citation Information

Cited By

  • Tactile sensor and preparation method and application thereof

    CN119935376A