A thermistor based on high entropy oxide and preparation method thereof
By using nano zinc oxide, nano zirconia, rare earth metal carbide and silicon carbide 6H-SiC, etc., the resistance deviation of NTC thermistor materials at high temperatures is solved. The major problem has achieved excellent high and low temperature impact performance and mechanical strength, meeting the needs of IGBT modules.
Patent Information
- Application Number
- CN202411132475.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing NTC thermistor materials have large resistance deviations in cycling resistance against high and low temperature impact at 25-600℃, which cannot meet the needs of IGBT modules.
Rare earth metal carbides with nano-silicon 6H-SiC and 6H-SiC and 6H-SiC of silicon carbides of 0.1-0.8 wt% nano-zinc oxide, 0.2-1.0 wt% nano-zirconia, 0.5-2.5 wt% nano-sheet structure, 20.0-40.0 wt% silicon carbide 6H-SiC and The amount is a high-entropy oxide-based thermistor made of high-entropy oxide ceramic powder. High-quality high-entropy oxide ceramic powder is prepared by specific sintering and ball milling treatment methods, and combined with surface single atom modified silicon carbide 6H- SiC, optimized resistance and mechanical strength.
The resistance deviation of the cyclic high and low temperature impact resistance performance at 25-600℃ is ≤0.8%, which meets the needs of the new generation of IGBT modules and improves the overall thermal stability and mechanical strength.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of NTC thermistors, in particular to a thermistor based on high entropy oxide. Background Art
[0002] High-entropy oxides refer to oxides composed of multiple metal elements, which have the characteristics of high entropy, good thermal stability, corrosion resistance, complex structure and diverse components, making them have broad application prospects in physics, chemistry, biology and other fields. NTC thermistor materials, that is, negative temperature coefficient thermistors, are usually solid solution materials composed of transition metal oxides. They show different resistance values at different temperatures. The higher the temperature, the lower the resistivity of the NTC thermistor material. It has the functions of temperature compensation and surge suppression, and has the advantages of high sensitivity, fast response speed and small size. It is widely used in daily life and industrial production.
[0003] NTC thermistor materials are mainly composed of metal oxides containing manganese (Mn), nickel (Ni), copper (Cu), iron (Fe), zinc (Zn), cobalt (Co) and other main components, while high entropy oxides can also use manganese (Mn), nickel (Ni), copper (Cu), iron (Fe), zinc (Zn), cobalt (Co) and other oxides as raw materials to produce five-element or six-element high entropy oxides. The formed five-element or six-element high entropy oxides can be used as NTC thermistor materials, which have good corrosion resistance and thermal stability, and improve the overall high and low temperature aging performance of NTC thermistor materials and the high temperature resistance drift rate under cyclic high and low temperature impact. For example, Chinese patent CN112802648A discloses a thermistor based on high entropy oxide. The thermistor is composed of oxides of five elements: cobalt, manganese, nickel, iron, and zinc. A single spinel phase high entropy oxide powder material is prepared by a high-temperature solid-phase chemical reaction. The prepared NTC thermistor (25°C) has a material constant B value of 6.5 to 12KΩ·cm and is 3500–3800K. After aging for 1000 hours at 125°C, the resistance drift rate is less than 0.05%, which can greatly improve the stability of the NTC thermistor.
[0004] With respect to the NTC thermistor materials in the above-mentioned prior art, the applicant found that the high and low temperature impact resistance performance of the cyclical high and low temperature impact resistance at 25-125°C can be controlled below 0.5%, but the resistance deviation of the high and low temperature impact resistance performance of the cyclical high and low temperature impact resistance at 25-600°C is 1.5-2.0%, which is relatively large and cannot meet the demand of the IGBT module for NTC thermistor materials. To this end, the present invention provides a thermistor based on high entropy oxide and a preparation method thereof. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a thermistor based on high entropy oxide and a preparation method thereof.
[0006] The present invention provides a thermistor based on high entropy oxide, which is realized by the following technical solutions:
[0007] A thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.1-0.8wt% of nano zinc oxide, 0.2-1.0wt% of nano zirconium oxide, 0.5-2.5wt% of rare earth metal carbide with nano sheet structure, 20.0-40.0wt% of silicon carbide 6H-SiC, and the balance is high entropy oxide ceramic micropowder; the rare earth metal carbide with nano sheet structure is niobium carbide nanosheet and / or tantalum carbide nanosheet; the high entropy oxide ceramic micropowder is a spinel-structured high entropy oxide ceramic micropowder formed by sintering and melting manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide and zirconium dioxide at a metal atomic molar ratio of 1:1:1:1:1, and ball milling.
[0008] Preferably, the high entropy oxide-based thermistor is made of the following raw materials in percentage by mass: 0.4-0.6wt% of nano zinc oxide, 0.6-0.8wt% of nano zirconium oxide, 1.8-2.4wt% of nanosheet structured rare earth metal carbide, 32-36wt% of silicon carbide 6H-SiC, and the remainder is high entropy oxide ceramic powder.
[0009] The invention has excellent high and low temperature impact performance under high temperature use environment, and the resistance deviation of the cyclic high and low temperature impact resistance performance at 25-600°C is ≤0.8%.
[0010] Preferably, the preparation method of the high entropy oxide ceramic powder is as follows:
[0011] S1: accurately weigh manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide and zirconium dioxide at a metal atomic molar ratio of Mn:Co:Ce:La:Zr=1:1:1:1:1, place them in a planetary ball mill for wet ball milling, the solid-liquid ratio is 1:(0.8-1.2), the grinding beads are tungsten carbide grinding beads, and the ball milling speed is adjusted to 80-120rpm under nitrogen protection for 200-240min, then adjusted to 300-320rpm for 60-80min, and then adjusted to 60-80rpm for 4-6h to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 90-95℃ and dried for 2-3h to obtain a mixed powder;
[0012] S2, placing the obtained mixed powder in a molding die and cold isostatically pressing at 200-300 MPa to obtain a preform, and placing the preform in a box-type high-temperature muffle furnace and heating it to 1180-1240° C. to sinter and melt for 8-12 hours to obtain a high entropy oxide ceramic part;
[0013] S3, placing the high entropy oxide ceramic product in a double-roll crusher for crushing to obtain high entropy oxide ceramic particles, and then placing the obtained high entropy oxide ceramic particles in a planetary ball mill for wet ball milling. A solvent is used in the wet ball milling, and the solid-liquid ratio of the solvent to the powder is 1: (0.8-1.2). The grinding beads are tungsten carbide grinding beads. Under nitrogen protection, the ball milling speed is adjusted to 300-400 rpm for ball milling for 120-180 min, and then the speed is adjusted to 60-80 rpm for ball milling for 30-60 min, and then the speed is adjusted to 160-180 rpm for ball milling for 2-4 h to obtain a wet mixture. The obtained wet mixture is placed in an oven, heated to 90-95 ° C and dried for 2-3 h to obtain high entropy oxide ceramic micropowder.
[0014] Preferably, the S1, with a metal atomic molar ratio of Mn:Co:Ce:La:Zr=1:1:1:1:1, accurately weigh manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide, and zirconium dioxide, and place them in a planetary ball mill, add a solvent formed by a mixture of ethanol and deionized water in a volume ratio of 1:1 for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and under nitrogen protection, the ball milling speed is adjusted to 120 rpm for ball milling for 200 min, then the speed is adjusted to 300 rpm for ball milling for 60 min, and then the speed is adjusted to 60 rpm for ball milling for 5 h to obtain a wet mixture, the obtained wet mixture is placed in an oven, heated to 90°C and dried for 2 h to obtain a mixed powder.
[0015] Preferably, in S3, the high entropy oxide ceramic product is placed in a double-roll crusher for crushing to obtain high entropy oxide ceramic particles, and the obtained high entropy oxide ceramic particles are placed in a planetary ball mill, and a solvent formed by a mixture of acetone and deionized water in a volume ratio of 1:4 is added for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and the ball milling speed is adjusted to 360 rpm under nitrogen protection for 150 min, then the speed is adjusted to 60 rpm for 30 min, and then the speed is adjusted to 160 rpm for 3 h to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 90°C and dried for 2 h to obtain a high entropy oxide ceramic powder.
[0016] The preparation method of the high entropy oxide ceramic micropowder provided by the present invention can not only ensure that high-quality and fine-grained high entropy oxide ceramic micropowder is obtained through processing, but also the overall preparation method is relatively simple, has strong feasibility, and is easy to realize industrial production and manufacturing.
[0017] Preferably, the rare earth metal carbide with nanosheet structure is composed of niobium carbide nanosheets and tantalum carbide nanosheets in a mass ratio of 1:(0.5-2).
[0018] By adopting the above technical solution, the overall heat-resistant stability and mechanical strength of the NTC thermistor can be improved.
[0019] Preferably, the silicon carbide 6H-SiC is surface single-atom modified silicon carbide 6H-SiC, and the surface single-atom modified silicon carbide 6H-SiC includes a silicon carbide 6H-SiC carrier and an active metal fixed on the surface of the silicon carbide 6H-SiC carrier in the form of a single atom, and the active metal is at least one of Mn, Co, Ni, Cu, Zn, Ce, Bi, Cr, La, Nb, and Ta; the content of the single-atom active metal doped in the surface of the surface single-atom modified silicon carbide 6H-SiC is 0.5-5wt%.
[0020] Preferably, the active metal is composed of Mn, Ni, Co, and La in a mass ratio of 1:1:1:(0.1-0.5); the content of single-atom active metal doped in the surface of the surface single-atom modified silicon carbide 6H-SiC is 2-2.5wt%.
[0021] By adopting the above technical solution, the resistance and B value of the NTC thermistor at 25°C can be finely controlled, and the overall heat resistance stability and mechanical strength can be effectively improved.
[0022] The present invention provides a method for preparing a thermistor based on high entropy oxide, which is achieved by the following scheme:
[0023] A method for preparing a thermistor based on high entropy oxide comprises the following steps:
[0024] Step 1, preparation of high entropy oxide ceramic powder;
[0025] Step 2, placing high entropy oxide ceramic powder, nano zinc oxide, nano zirconium oxide, rare earth metal carbide with nano sheet structure, and silicon carbide 6H-SiC in a planetary ball mill for wet ball milling, wherein a solvent is used in the wet ball milling process, and the solid-liquid ratio of the solvent to the powder is 1:(0.8-1.2), and the grinding beads are tungsten carbide grinding beads. Under nitrogen protection, the ball milling speed is adjusted to 60-80rpm and the ball milling is performed for 2-4 hours to obtain a wet mixture, and the obtained wet mixture is placed in an oven and heated to 80-85°C and dried for 2-4 hours to obtain a mixed powder;
[0026] Step 3, the obtained mixed powder is placed in a molding mold for cold isostatic pressing to obtain an NTC ceramic preform;
[0027] Step 4, the NTC ceramic preform in step 3 is subjected to rapid sintering treatment, firstly the temperature is raised to 1100-1180°C and kept for 1-3h, then the temperature is raised to 1650-1680°C and kept for 1-3h, then the temperature is raised to 2180-2250°C and kept for 0.5-1h, and finally the temperature is lowered to 800-850°C, and the semi-finished NTC thermistor material is obtained after the furnace is opened and naturally cooled to room temperature;
[0028] Step 5: De-stress the semi-finished NTC thermistor material obtained in step 4 by first heating it to 200-240°C and keeping it for 1-2 hours under an inert atmosphere, then heating it to 400-420°C at a rate of 40-80°C / min and keeping it for 4-8 hours, and finally opening the furnace and naturally cooling it to room temperature to obtain a finished high entropy oxide-based thermistor.
[0029] Preferably, in the step three, the obtained mixed powder is placed in a molding mold for cold isostatic pressing treatment, the molding temperature is 20-50°C, and the molding pressure is: first pressurized to 200MPa at 10MPa / s, maintained for 60s, then pressurized to 360MPa at 5MPa / s, maintained for 180s, then reduced to 200MPa at 5MPa / s, maintained for 30s, and then reduced to 0MPa at 20MPa / s. The molding speed is 0.5mm / s. After completing the cold isostatic pressing treatment, the NTC ceramic preform can be obtained.
[0030] The preparation method provided by the present invention is relatively simple, has relatively low operating difficulty, and is easy to implement industrial production.
[0031] In summary, the present invention has the following advantages:
[0032] 1. The present invention has excellent high and low temperature impact performance and relatively good mechanical strength under high temperature use environment, and the resistance deviation of the cyclic high and low temperature impact resistance at 25-600°C is ≤0.8%, which meets the use requirements of the new generation of IGBT modules.
[0033] 2. The preparation method of high entropy oxide ceramic micropowder provided by the present invention can not only ensure the processing to obtain high-quality and fine-grained high entropy oxide ceramic micropowder, but also the overall preparation method is relatively simple, has strong feasibility, and is easy to realize industrial production and manufacturing.
[0034] 3. In the present invention, the surface of silicon carbide 6H-SiC is modified by single-atom doping. Under the premise of ensuring the overall heat-resistant stability and mechanical strength, the resistivity and B value of the NTC thermistor (25°C) can be adjusted.
[0035] 4. The preparation method of the thermistor based on high entropy oxide provided by the present invention is relatively simple, the production equipment is standardized production, the production input cost is relatively low, and the operation difficulty is relatively low, which is convenient for industrial production and manufacturing. DETAILED DESCRIPTION
[0036] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.
[0037] Preparation Example
[0038] Preparation Example 1: The preparation method of high entropy oxide ceramic powder is as follows:
[0039] S1, accurately weigh manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide, and zirconium dioxide at a metal atomic molar ratio of Mn:Co:Ce:La:Zr=1:1:1:1:1, place them in a planetary ball mill, add a solvent formed by mixing ethanol and deionized water in a volume ratio of 1:1 for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and under nitrogen protection, the ball milling speed is adjusted to 120 rpm for ball milling for 200 min, then the speed is adjusted to 300 rpm for ball milling for 60 min, and then the speed is adjusted to 60 rpm for ball milling for 5 h to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 90°C and dried for 2 h to obtain a mixed powder;
[0040] S2, placing the obtained mixed powder in a molding die and cold isostatically pressing at 300 MPa to obtain a preform, and placing the preform in a box-type high-temperature muffle furnace and heating it to 1180° C. to sinter and melt for 12 hours to obtain a high entropy oxide ceramic part;
[0041] S3, placing the high entropy oxide ceramic part in a double-roll crusher for crushing to obtain high entropy oxide ceramic particles, then placing the obtained high entropy oxide ceramic particles in a planetary ball mill, adding a solvent formed by a mixture of acetone and deionized water in a volume ratio of 1:4 for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and under nitrogen protection, the ball milling speed is adjusted to 360 rpm for ball milling for 150 min, then the speed is adjusted to 60 rpm for ball milling for 30 min, and then the speed is adjusted to 160 rpm for ball milling for 3 h to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 90°C and dried for 2 h to obtain a high entropy oxide ceramic micropowder.
[0042] The difference between Preparation Example 2 and Preparation Example 1 is that: S2, the obtained mixed powder is placed in a molding mold and cold isostatically pressed at 300 MPa to obtain a preform, and the preform is placed in a box-type high-temperature muffle furnace and heated to 1200°C and sintered and melted for 10 hours to obtain a high-entropy oxide ceramic part.
[0043] The difference between Preparation Example 3 and Preparation Example 1 is that: S2, the obtained mixed powder is placed in a molding mold and cold isostatically pressed at 300 MPa to obtain a preform, and the preform is placed in a box-type high-temperature muffle furnace and heated to 1240°C and sintered and melted for 8 hours to obtain a high-entropy oxide ceramic part.
[0044] The difference between Preparation Example 4 and Preparation Example 1 is that: S2, the obtained mixed powder is placed in a molding mold and cold isostatically pressed at 300 MPa to obtain a preform, and the preform is placed in a box-type high-temperature muffle furnace and heated to 1100°C and sintered and melted for 12 hours to obtain a high-entropy oxide ceramic part.
[0045] Preparation Example 5: A preparation method of a negative temperature coefficient thermistor based on high entropy oxide is as follows:
[0046] a. Accurately weigh manganese tetraoxide, cobalt tetraoxide, nickel oxide, ferric oxide and zinc oxide according to Co:Mn:Fe:Ni:Zn=1:1:1:1:1, put them into a ball mill, add a solvent, the volume ratio of deionized water and anhydrous ethanol in the solvent is 1:1, place the ball mill in a planetary ball mill, grind for 10 hours to obtain a mixture;
[0047] b. Drying the mixture in step a in an oven at 85° C., and then heating at 1100° C. for 15 h to melt the mixture into a single spinel structure high entropy oxide material;
[0048] c. Grind the high entropy oxide powder material obtained in step b for a second time in a planetary ball mill for 10 hours and dry to obtain a powder;
[0049] d. Pre-press the powder obtained in step c, and then perform isostatic pressing, the pressure of which is controlled at 350 MPa and maintained for 5 minutes;
[0050] e. Sinter the isostatically pressed block obtained in step d at 1200° C. for 6 h to obtain a high-entropy oxide ceramic product, place the high-entropy oxide ceramic product in a double-roll crusher for crushing to obtain high-entropy oxide ceramic particles, and then place the obtained high-entropy oxide ceramic particles in a planetary ball mill, add a solvent formed by a mixture of acetone and deionized water in a volume ratio of 1:4 for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and under nitrogen protection, the ball milling speed is adjusted to 360 rpm for ball milling for 150 min, then the speed is adjusted to 60 rpm for ball milling for 30 min, and then the speed is adjusted to 160 rpm for ball milling for 3 h to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 90° C. and dried for 2 h to obtain a high-entropy oxide ceramic powder.
[0051] Example
[0052] A thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.1-0.8wt% of nano zinc oxide, 0.2-1.0wt% of nano zirconium oxide, 0.5-2.5wt% of rare earth metal carbide with nano sheet structure, 20.0-40.0wt% of silicon carbide 6H-SiC, and the balance is high entropy oxide ceramic powder.
[0053] Preferably, the high entropy oxide based thermistor is made of the following raw materials in percentage by mass: 0.4-0.6wt% of nano zinc oxide, 0.6-0.8wt% of nano zirconium oxide, 1.8-2.4wt% of rare earth metal carbide with nanosheet structure, 32-36wt% of silicon carbide 6H-SiC, and the remainder is high entropy oxide ceramic powder.
[0054] The rare earth metal carbide with nanosheet structure is niobium carbide nanosheet and / or tantalum carbide nanosheet. Preferably, the rare earth metal carbide with nanosheet structure is composed of niobium carbide nanosheet and tantalum carbide nanosheet in a mass ratio of 1:(0.5-2).
[0055] Preferably, silicon carbide 6H-SiC is surface single-atom modified silicon carbide 6H-SiC. Surface single-atom modified silicon carbide 6H-SiC includes a silicon carbide 6H-SiC carrier and an active metal fixed on the surface of the silicon carbide 6H-SiC carrier in the form of a single atom. The active metal is at least one of Mn, Co, Ni, Cu, Zn, Ce, Bi, Cr, La, Nb, and Ta. The content of doped single-atom active metal in the surface of the surface single-atom modified silicon carbide 6H-SiC is 0.5-5wt%. Further preferably, the active metal is composed of Mn, Ni, Co, and La in a mass ratio of 1:1:1:(0.1-0.5) and the content of doped single-atom active metal in the surface of the surface single-atom modified silicon carbide 6H-SiC is 2-2.5wt%.
[0056] The preparation method of high entropy oxide ceramic powder is as follows:
[0057] S1, accurately weigh manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide, and zirconium dioxide with a metal atomic molar ratio of Mn:Co:Ce:La:Cr=1:1:1:1:1, place them in a planetary ball mill for wet ball milling, use a solvent in the wet ball milling, and the solid-liquid ratio of the solvent to the powder is 1:(0.8-1.2), the grinding beads are tungsten carbide grinding beads, and adjust the ball milling speed to 80-120rpm under nitrogen protection for 200-240min, then adjust the speed to 300-320rpm for 60-80min, and then adjust the speed to 60-80rpm for 4-6h to obtain a wet mixture, place the obtained wet mixture in an oven, heat it to 90-95℃, and dry it for 2-3h to obtain a mixed powder;
[0058] Preferably, S1, accurately weigh manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide, and zirconium dioxide in a metal atomic molar ratio of Mn:Co:Ce:La:Zr=1:1:1:1:1, place them in a planetary ball mill, add a solvent formed by mixing ethanol and deionized water in a volume ratio of 1:1 for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and the ball milling speed is adjusted to 120rpm under nitrogen protection for 200min, then the speed is adjusted to 300rpm for 60min, and then the speed is adjusted to 60rpm for 5h to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 90°C and dried for 2h to obtain a mixed powder;
[0059] S2, placing the obtained mixed powder in a molding die and cold isostatically pressing at 200-300 MPa to obtain a preform, and placing the preform in a box-type high-temperature muffle furnace and heating it to 1180-1240° C. to sinter and melt for 8-12 hours to obtain a high entropy oxide ceramic part;
[0060] S3, placing the high entropy oxide ceramic part in a double-roll crusher for crushing to obtain high entropy oxide ceramic particles, and then placing the obtained high entropy oxide ceramic particles in a planetary ball mill for wet ball milling, with a solid-liquid ratio of 1: (0.8-1.2), and the grinding beads are tungsten carbide grinding beads. Under nitrogen protection, the ball milling speed is adjusted to 300-400 rpm for ball milling for 120-180 min, and then the speed is adjusted to 60-80 rpm for ball milling for 30-60 min, and then the speed is adjusted to 160-180 rpm for ball milling for 2-4 h to obtain a wet mixture, and the obtained wet mixture is placed in an oven and heated to 90-95 ° C. and dried for 2-3 h to obtain high entropy oxide ceramic powder;
[0061] Preferably, S3, placing the high-entropy oxide ceramic product in a double-roll crusher for crushing to obtain high-entropy oxide ceramic particles, then placing the obtained high-entropy oxide ceramic particles in a planetary ball mill, adding a solvent formed by a mixture of acetone and deionized water in a volume ratio of 1:4 for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and the ball milling speed is adjusted to 360rpm under nitrogen protection for ball milling for 150min, then the speed is adjusted to 60rpm for ball milling for 30min, and then the speed is adjusted to 160rpm for ball milling for 3h to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 90°C and dried for 2h to obtain a high-entropy oxide ceramic powder.
[0062] A method for preparing a thermistor based on high entropy oxide comprises the following steps:
[0063] Step 1, preparation of high entropy oxide ceramic powder;
[0064] Step 2, placing high entropy oxide ceramic powder, nano zinc oxide, nano zirconium oxide, rare earth metal carbide with nano sheet structure, and silicon carbide 6H-SiC in a planetary ball mill for wet ball milling, with a solid-liquid ratio of 1: (0.8-1.2), and using tungsten carbide grinding beads. Adjust the ball mill speed to 60-80 rpm under nitrogen protection for 2-4 hours to obtain a wet mixture, and place the obtained wet mixture in an oven, heat it to 80-85° C., and dry it for 2-4 hours to obtain a mixed powder;
[0065] Step three, step three, the obtained mixed powder is placed in a molding mold for cold isostatic pressing, the molding temperature is 20-50°C, the molding pressure is: first pressurized to 200MPa at 10MPa / s, maintained for 60s, then pressurized to 360MPa at 5MPa / s, maintained for 180s, then reduced to 200MPa at 5MPa / s, maintained for 30s, then reduced to 0MPa at 20MPa / s, the molding speed is 0.5mm / s, and the NTC ceramic preform can be obtained after the cold isostatic pressing treatment is completed;
[0066] Step 4, the NTC ceramic preform in step 3 is subjected to rapid sintering treatment, firstly the temperature is raised to 1100-1180°C and kept for 1-3h, then the temperature is raised to 1650-1680°C and kept for 1-3h, then the temperature is raised to 2180-2250°C and kept for 0.5-1h, and finally the temperature is lowered to 800-850°C, and the semi-finished NTC thermistor material is obtained after the furnace is opened and naturally cooled to room temperature;
[0067] Step 5: De-stress the semi-finished NTC thermistor material obtained in step 4 by first heating it to 200-240°C and keeping it for 1-2 hours under an inert atmosphere, then heating it to 400-420°C at a rate of 40-80°C / min and keeping it for 4-8 hours, and finally opening the furnace and naturally cooling it to room temperature to obtain a finished high entropy oxide-based thermistor.
[0068] Example 1: A thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.5wt% of nano zinc oxide (model CW-ZnO-002, particle size 200nm, Shanghai Chaowei Nano Technology), 0.8wt% of nano zirconium oxide (model CW-ZrO2-002, particle size 50nm, 3Y tetragonal phase crystal, Shanghai Chaowei Nano Technology), 1.0wt% of niobium carbide nanosheets (niobium carbide (Nb2CTx) MXene multilayer nanosheets, sheet diameter: 1-10μm thickness: 100-300nm, Zhongke Leiming (Beijing) Technology), 1.2wt% of tantalum carbide nanosheets, 34wt% of silicon carbide 6H-SiC (customized by Xi'an Qiyue Biotechnology Co., Ltd., average particle size 0.5-1μm), and the remainder is the high entropy oxide ceramic micropowder in Preparation Example 1.
[0069] A method for preparing a thermistor based on high entropy oxide comprises the following steps:
[0070] Step 1: Preparation of high entropy oxide ceramic powder, see the preparation of high entropy oxide ceramic powder in Preparation Example 1;
[0071] Step 2: placing high entropy oxide ceramic powder, nano zinc oxide, nano zirconium oxide, niobium carbide nanosheets, tantalum carbide nanosheets, and silicon carbide 6H-SiC in a planetary ball mill, adding a solvent formed by mixing ethanol and deionized water in a volume ratio of 1:1 for wet ball milling, the solid-liquid ratio is 1:1, the grinding beads are tungsten carbide grinding beads, and the ball milling speed is adjusted to 60 rpm under nitrogen protection for 4 hours to obtain a wet mixture, and the obtained wet mixture is placed in an oven, heated to 85° C. and dried for 4 hours to obtain a mixed powder;
[0072] Step 3, the obtained mixed powder is placed in a molding mold for cold isostatic pressing, the molding temperature is 25°C, the molding pressure is: first pressurized to 200MPa at 10MPa / s, maintained for 60s, then pressurized to 360MPa at 5MPa / s, maintained for 180s, then reduced to 200MPa at 5MPa / s, maintained for 30s, then reduced to 0MPa at 20MPa / s, the molding speed is 0.5mm / s, and the NTC ceramic preform can be obtained after the cold isostatic pressing treatment is completed;
[0073] Step 4, the NTC ceramic preform in step 3 is subjected to rapid sintering treatment, firstly the temperature is raised to 1180°C at 50°C / min and kept at this temperature for 2h, then the temperature is raised to 1650°C at 100°C / min and kept at this temperature for 1h, then the temperature is raised to 2200°C at 200°C / min and kept at this temperature for 1h, and finally the temperature is cooled to 820°C at 50°C / min by air cooling, and the furnace is opened and naturally cooled to room temperature to obtain a semi-finished NTC thermistor material;
[0074] Step 5: De-stress the semi-finished NTC thermistor material obtained in step 4 by first heating the material to 240°C at 20°C / min and keeping it for 2h in an inert atmosphere, then heating the material to 400°C at 50°C / min and keeping it for 8h. Finally, the material is naturally cooled to room temperature to obtain a finished product high entropy oxide-based thermistor.
[0075] The difference between Example 2 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.2wt% of nano zinc oxide, 0.5wt% of nano zirconium oxide, 0.3wt% of niobium carbide nanosheets, 0.2wt% of tantalum carbide nanosheets, 20wt% of silicon carbide 6H-SiC, and the remainder is the high entropy oxide ceramic powder in Preparation Example 1.
[0076] The difference between Example 3 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.8wt% of nano zinc oxide, 1wt% of nano zirconium oxide, 1.5wt% of niobium carbide nanosheets, 1.0wt% of tantalum carbide nanosheets, 40wt% of silicon carbide 6H-SiC, and the remainder is the high entropy oxide ceramic powder in Preparation Example 1.
[0077] The difference between Example 4 and Example 1 is that the high entropy oxide ceramic powder in Preparation Example 1 is replaced by the high entropy oxide ceramic powder in Preparation Example 2.
[0078] The difference between Example 5 and Example 1 is that the high entropy oxide ceramic powder in Preparation Example 1 is replaced by the high entropy oxide ceramic powder in Preparation Example 3.
[0079] The difference between Example 6 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.5wt% of nano zinc oxide, 0.8wt% of nano zirconium oxide, 2.2wt% of niobium carbide nanosheets, 34wt% of silicon carbide 6H-SiC, and the remainder is the high entropy oxide ceramic powder in Preparation Example 1.
[0080] The difference between Example 7 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.5wt% of nano zinc oxide, 0.8wt% of nano zirconium oxide, 2.2wt% of tantalum carbide nanosheets, 34wt% of silicon carbide 6H-SiC, and the remainder is the high entropy oxide ceramic powder in Preparation Example 1.
[0081] The difference between Example 8 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by weight: 0.5wt% nano zinc oxide, 0.8wt% nano zirconium oxide, 1.1wt%
[0082] % niobium carbide nanosheets, 1.1wt% tantalum carbide nanosheets, 34wt% silicon carbide 6H-SiC, and the balance being the high entropy oxide ceramic powder in Preparation Example 1.
[0083] The difference between Example 9 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.5wt% of nano zinc oxide, 0.8wt% of nano zirconium oxide, 1.5wt% of niobium carbide nanosheets, 0.7wt% of tantalum carbide nanosheets, 34wt% of silicon carbide 6H-SiC, and the remainder is the high entropy oxide ceramic powder in Preparation Example 1.
[0084] The difference between Example 10 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.5wt% of nano zinc oxide, 0.8wt% of nano zirconium oxide, 0.7wt% of niobium carbide nanosheets, 1.5wt% of tantalum carbide nanosheets, 34wt% of silicon carbide 6H-SiC, and the remainder is the high entropy oxide ceramic powder in Preparation Example 1.
[0085] The difference between Example 11 and Example 1 is that silicon carbide 6H-SiC is surface single-atom modified silicon carbide 6H-SiC. Surface single-atom modified silicon carbide 6H-SiC includes a silicon carbide 6H-SiC carrier and an active metal fixed on the surface of the silicon carbide 6H-SiC carrier in the form of a single atom. The active metals are Mn, Co, Ni, and Zn, and the mass ratio of Mn, Co, Ni, and Zn is 1:1:1:1. The content of single-atom active metal doped in the surface of the surface single-atom modified silicon carbide 6H-SiC is 2.65wt%.
[0086] The preparation method of surface single atom modified silicon carbide 6H-SiC is as follows:
[0087] Step 1: prepare 1L of 20wt% citric acid aqueous solution, weigh 100g of silicon carbide 6H-SiC and soak it in 20wt% citric acid aqueous solution for 6h, take it out and dry it for later use;
[0088] At the same time, 2.43 g of manganese dichloride tetrahydrate, 2.73 g of cobalt dichloride hexahydrate, 2.76 g of nickel dichloride hexahydrate, and 1.41 g of zinc chloride were dissolved in 500 mL of deionized water to obtain a metal impregnation solution.
[0089] Step 2: immerse 100 g of the citric acid-treated silicon carbide 6H-SiC carrier in a metal impregnation solution, perform ultrasonic dispersion treatment at an ultrasonic frequency of 44 kHz and an ultrasonic power of 1200 W for 8 h, mechanically stir at 320 rpm for 24 h, then remove the supernatant, centrifuge and separate the solid material, place it in a 120° C. forced drying oven and dry it for 12 h to obtain a solid material;
[0090] Step three, after drying, the obtained solid material is placed in a planetary ball mill and ball-milled at 120 rpm for 30 minutes to obtain a solid powder, the obtained solid powder is heated to 540°C at 5°C / min under an argon atmosphere, and the calcination time is 4 hours, and the obtained solid material is placed in a planetary ball mill and ball-milled at 80 rpm for 60 minutes to obtain a particle size of 0.5-1 μm surface single atom modified silicon carbide 6H-SiC, and the total mass of the doped single atom active metal is 2.63wt%.
[0091] The difference between Example 12 and Example 1 is that the content of single-atom active metal doped in the surface of the surface single-atom modified silicon carbide 6H-SiC is 1 wt %.
[0092] The difference between Example 13 and Example 1 is that the content of single-atom active metal doped in the surface of the surface single-atom modified silicon carbide 6H-SiC is 5wt%.
[0093] The difference between Example 14 and Example 1 is that the content of single-atom active metal doped on the surface of the surface single-atom modified silicon carbide 6H-SiC is 2.5wt%. The active metal is composed of Mn, Ni, Co, and La in a mass ratio of 1:1:1:0.4.
[0094] The preparation method of surface single atom modified silicon carbide 6H-SiC is as follows:
[0095] Step 1: prepare 1L of 20wt% citric acid aqueous solution, weigh 100g of silicon carbide 6H-SiC and soak it in 20wt% citric acid aqueous solution for 6h, take it out and dry it for later use;
[0096] At the same time, 3.61 g of manganese dichloride tetrahydrate, 4.05 g of cobalt dichloride hexahydrate, 4.04 g of nickel dichloride hexahydrate, and 0.71 g of lanthanum chloride were dissolved in 500 mL of deionized water to obtain a metal impregnation solution.
[0097] Step 2: immerse 100 g of the citric acid-treated silicon carbide 6H-SiC carrier in a metal impregnation solution, perform ultrasonic dispersion treatment at an ultrasonic frequency of 44 kHz and an ultrasonic power of 1200 W for 8 h, mechanically stir at 320 rpm for 24 h, then remove the supernatant, centrifuge and separate the solid material, place it in a 120° C. forced drying oven and dry it for 12 h to obtain a solid material;
[0098] Step three, after drying, the obtained solid material is placed in a planetary ball mill and ball-milled at 120 rpm for 30 minutes to obtain a solid powder, the obtained solid powder is heated to 540°C at 5°C / min under an argon atmosphere, and the calcination time is 4 hours, and the obtained solid material is placed in a planetary ball mill and ball-milled at 80 rpm for 60 minutes to obtain a particle size of 0.5-1 μm surface single atom modified silicon carbide 6H-SiC, the total mass of doped single atom active metal is 3.28wt%.
[0099] The difference between Comparative Example 1 and Example 1 is that the high entropy oxide ceramic powder in Preparation Example 1 is replaced by the high entropy oxide ceramic powder in Preparation Example 4.
[0100] The difference between Comparative Example 2 and Example 1 is that the high entropy oxide ceramic powder in Preparation Example 1 is replaced by the high entropy oxide ceramic powder in Preparation Example 5.
[0101] The difference between Comparative Example 3 and Example 1 is that a thermistor based on high entropy oxide is made of the following raw materials in percentage by mass: 0.5wt% of nano zinc oxide, 0.8wt% of nano zirconium oxide, 34wt% of silicon carbide 6H-SiC, and the remainder is the high entropy oxide ceramic powder in Preparation Example 1.
[0102] The difference between Comparative Example 4 and Example 1 is that silicon carbide 6H-SiC is replaced by silicon carbide 3C-SiC.
[0103] The difference between Comparative Example 5 and Example 1 is that the thermistor based on high entropy oxide is made from the high entropy oxide ceramic powder in Preparation Example 1. The preparation method of the thermistor based on high entropy oxide is as follows: first, the high entropy oxide ceramic powder in Preparation Example 1 is placed in a molding mold for cold isostatic pressing, the molding temperature is 25°C, the molding pressure is: first pressurized to 200MPa at 10MPa / s, maintained for 60s, then pressurized to 360MPa at 5MPa / s, maintained for 180s, then reduced to 200MPa at 5MPa / s, maintained for 30s, then reduced to 0MPa at 20MPa / s, the molding speed is 0.5mm / s, and the NTC ceramic preform can be obtained after the cold isostatic pressing is completed. The NTC ceramic preform is then subjected to rapid sintering treatment, the temperature is increased to 1180°C at 50°C / min and kept for 4 hours, the temperature is reduced to 820°C at 50°C / min by air cooling, and the furnace is opened and naturally cooled to room temperature to obtain a semi-finished NTC thermistor material; finally, the semi-finished NTC thermistor material obtained in step 4 is subjected to stress relief treatment, the temperature is first increased to 240°C at 20°C / min and kept for 2 hours in an inert atmosphere, and then the temperature is increased to 400°C at 50°C / min and kept for 8 hours, and finally the furnace is opened and naturally cooled to room temperature to obtain a finished product based on high entropy oxide Thermistor.
[0104] The difference between Comparative Example 6 and Comparative Example 5 is that the high entropy oxide-based thermistor is made of the high entropy oxide ceramic powder in Preparation Example 5.
[0105] Performance test: NTC thermistor discs with a diameter of 10 mm and a thickness of 2 mm were prepared by using the formula and process in Examples 1-14 and Comparative Examples 1-6. After silver paste electrodes were coated on both ends, they were placed in a muffle furnace at 750°C for 30 minutes to obtain the NTC thermistor to be tested. The prepared NTC thermistor to be tested was heated to 600°C in a muffle furnace and tested for electrical properties using a Keithley 2600B multi-channel test system in the United States, and the B 25 / 600 . B value calculation formula: B T1 / T2 = [(T1*T2) / (T2-T1)]*ln(R T1 / R T2), where T1 and T2 are both Kelvin temperatures.
[0106] High and low temperature impact resistance test: The NTC thermistor to be tested is heated from 25℃ to 600℃ for 1000 cycles, and the test obtains R 0次 / 25℃ , R 0次 / 600℃ , R 1000次 / 25℃ , R 1000次 / 600℃ , ∆R 25℃ (absolute value) = | (R 0次 / 25℃ -R 1500次 / 25℃ ) / R 0次 / 25℃| ; ∆R 600℃ (absolute value) = |(R 0次 / 600℃ -R 1000次 / 600℃ ) / R 0次 / 600℃ |. R 0次 / 25℃ is the initial resistance value at 25°C; R 0次 / 600℃ is the resistance value when the temperature is first raised to 600°C; R 1000次 / 25℃ It is the resistance value measured at 25°C after 1000 cycles from 25°C to 600°C. 1000次 / 600℃ The resistance value is measured after heating from 25°C to 600°C for 1000 cycles and then heating to 600°C.
[0107] Table 1: Test parameter table of thermistors based on high entropy oxide in Examples 1-14 and Comparative Examples 1-6
[0108]
[0109] It can be seen from Examples 1-5 and Comparative Examples 1-2 and Table 1 that the NTC high entropy oxide thermistor prepared using the high entropy oxide ceramic powder in Preparation Examples 1-3 of the present invention has excellent high and low temperature impact performance, and the resistance deviation of the cyclic high and low temperature impact performance at 25-600°C is ≤0.8%.
[0110] It can be seen from Examples 1-5 and Comparative Example 3 and Table 1 that the addition of niobium carbide nanosheets and tantalum carbide nanosheets can improve the high and low temperature impact properties of the prepared NTC high entropy oxide thermistor material.
[0111] It can be seen from Examples 1-5 and Comparative Example 4 and Table 1 that the use of silicon carbide 6H-SiC can improve the resistivity, sensitivity and high and low temperature impact performance of the prepared NTC high entropy oxide thermistor material.
[0112] It can be seen from Examples 1-5 and Comparative Examples 5-6 and Table 1 that the NTC high entropy oxide thermistor material prepared by the thermistor formula based on high entropy oxide provided in the present invention has better sensitivity and high and low temperature impact performance than the thermistor material prepared from pure high entropy oxide, and the overall mechanical strength is also better.
[0113] It can be seen from Example 1 and Examples 6-10 and Table 1 that the high and low temperature impact performance of the prepared NTC high entropy oxide thermistor material is better when niobium carbide nanosheets and tantalum carbide nanosheets are used in combination. Preferably, niobium carbide nanosheets and tantalum carbide nanosheets form a rare earth metal carbide nanosheet structure in a mass ratio of 1:1.
[0114] It can be seen from Example 1 and Examples 11-14 and Table 1 that the resistivity and B value of the NTC thermistor (25°C) can be adjusted by performing surface single-atom doping modification treatment on silicon carbide 6H-SiC while ensuring the overall heat-resistant stability and mechanical strength.
[0115] In summary, the present invention has excellent high and low temperature impact performance under high temperature use environment, and the resistance deviation of the cyclic high and low temperature impact resistance at 25-600°C is ≤0.8%.
[0116] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.
Claims
1. A thermistor based on high entropy oxide, characterized in that: The thermistor is made of the following raw materials in percentage by mass: 0.1-0.8wt% of nano zinc oxide, 0.2-1.0wt% of nano zirconium oxide, 0.5-2.5wt% of rare earth metal carbide with a nanosheet structure, 20.0-40.0wt% of silicon carbide 6H-SiC, and the balance is high entropy oxide ceramic micropowder; the rare earth metal carbide with a nanosheet structure is niobium carbide nanosheet and / or tantalum carbide nanosheet; the high entropy oxide ceramic micropowder is a spinel structure high entropy oxide ceramic micropowder formed by sintering and melting manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide, and zirconium dioxide at a metal atomic molar ratio of 1:1:1:1:1, and ball milling and crushing; The preparation method of the high entropy oxide ceramic powder is as follows: S1, accurately weigh manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide, and zirconium dioxide with a metal atomic molar ratio of Mn:Co:Ce:La:Zr=1:1:1:1:1, place them in a planetary ball mill for wet ball milling, use a solvent in the wet ball milling, and the solid-liquid ratio of the solvent to the powder is 1:(0.8-1.2), the grinding beads are tungsten carbide grinding beads, and adjust the ball milling speed to 80-120rpm under nitrogen protection for 200-240min, then adjust the speed to 300-320rpm for 60-80min, and then adjust the speed to 60-80rpm for 4-6h to obtain a wet mixture, place the obtained wet mixture in an oven, heat it to 90-95℃, and dry it for 2-3h to obtain a mixed powder; S2, placing the obtained mixed powder in a molding die and cold isostatically pressing at 200-300 MPa to obtain a preform, and placing the preform in a box-type high-temperature muffle furnace and heating it to 1180-1240° C. to sinter and melt for 8-12 hours to obtain a high entropy oxide ceramic part; S3, placing the high entropy oxide ceramic product in a double-roll crusher for crushing to obtain high entropy oxide ceramic particles, and then placing the obtained high entropy oxide ceramic particles in a planetary ball mill for wet ball milling. A solvent is used in the wet ball milling, and the solid-liquid ratio of the solvent to the powder is 1: (0.8-1.2). The grinding beads are tungsten carbide grinding beads. Under nitrogen protection, the ball milling speed is adjusted to 300-400 rpm for ball milling for 120-180 min, and then the speed is adjusted to 60-80 rpm for ball milling for 30-60 min, and then the speed is adjusted to 160-180 rpm for ball milling for 2-4 h to obtain a wet mixture. The obtained wet mixture is placed in an oven, heated to 90-95 ° C and dried for 2-3 h to obtain high entropy oxide ceramic micropowder.
2. A thermistor based on high entropy oxide according to claim 1, characterized in that: The S1, with a metal atomic molar ratio of Mn:Co:Ce:La:Zr=1:1:1:1:1, accurately weigh manganese tetraoxide, cobalt tetraoxide, cerium dioxide, lanthanum trioxide, and zirconium dioxide, and place them in a planetary ball mill. A solvent formed by a mixture of ethanol and deionized water in a volume ratio of 1:1 is added for wet ball milling. The solid-liquid ratio is 1:1.2, and the grinding beads are tungsten carbide grinding beads. Under nitrogen protection, the ball milling speed is adjusted to 120 rpm for ball milling for 200 min, then adjusted to 300 rpm for ball milling for 60 min, and then adjusted to 60 rpm for ball milling for 5 h to obtain a wet mixture. The obtained wet mixture is placed in an oven, heated to 90°C and dried for 2 h to obtain a mixed powder.
3. A thermistor based on high entropy oxide according to claim 2, characterized in that: The S3 is to place the high entropy oxide ceramic part in a double-roll crusher for crushing to obtain high entropy oxide ceramic particles, and then place the obtained high entropy oxide ceramic particles in a planetary ball mill, add a solvent formed by mixing acetone and deionized water in a volume ratio of 1:4 for wet ball milling, the solid-liquid ratio is 1:1.2, the grinding beads are tungsten carbide grinding beads, and adjust the ball milling speed to 360rpm under nitrogen protection for ball milling for 150min, then adjust the speed to 60rpm for ball milling for 30min, and then adjust the speed to 160rpm for ball milling for 3h to obtain a wet mixture, place the obtained wet mixture in an oven, heat it to 90°C and dry it for 2h to obtain high entropy oxide ceramic micropowder.
4. The high entropy oxide based thermistor according to claim 1, characterized in that: The high entropy oxide-based thermistor is made of the following raw materials in percentage by mass: 0.4-0.6wt% of nano zinc oxide, 0.6-0.8wt% of nano zirconium oxide, 1.8-2.4wt% of rare earth metal carbide with a nanosheet structure, 32-36wt% of silicon carbide 6H-SiC, and the remainder is high entropy oxide ceramic powder.
5. A thermistor based on high entropy oxide according to claim 4, characterized in that: The rare earth metal carbide with nanosheet structure is composed of niobium carbide nanosheets and tantalum carbide nanosheets in a mass ratio of 1:(0.5-2).
6. The high entropy oxide based thermistor according to claim 5, characterized in that: The silicon carbide 6H-SiC is surface single-atom modified silicon carbide 6H-SiC, and the surface single-atom modified silicon carbide 6H-SiC includes a silicon carbide 6H-SiC carrier and an active metal fixed on the surface of the silicon carbide 6H-SiC carrier in the form of a single atom, and the active metal is at least one of Mn, Co, Ni, Cu, Zn, Ce, Bi, Cr, La, Nb, and Ta; and the content of the single-atom active metal doped in the surface of the surface single-atom modified silicon carbide 6H-SiC is 0.5-5wt%.
7. A thermistor based on high entropy oxide according to claim 6, characterized in that: The active metal is composed of Mn, Ni, Co, and La in a mass ratio of 1:1:1:(0.1-0.5); the content of the single-atom active metal doped on the surface of the surface single-atom modified silicon carbide 6H-SiC is 2-2.5wt%.
8. A method for preparing a thermistor based on a high entropy oxide according to any one of claims 1 to 7, characterized in that: The following steps are involved: Step 1, preparation of high entropy oxide ceramic powder; Step 2, placing high entropy oxide ceramic powder, nano zinc oxide, nano zirconium oxide, rare earth metal carbide with nano sheet structure, and silicon carbide 6H-SiC in a planetary ball mill for wet ball milling, wherein a solvent is used in the wet ball milling process, and the solid-liquid ratio of the solvent to the powder is 1:(0.8-1.2), and the grinding beads are tungsten carbide grinding beads. Under nitrogen protection, the ball milling speed is adjusted to 60-80rpm and the ball milling is performed for 2-4 hours to obtain a wet mixture, and the obtained wet mixture is placed in an oven and heated to 80-85°C and dried for 2-4 hours to obtain a mixed powder; Step 3, the obtained mixed powder is placed in a molding mold for cold isostatic pressing to obtain an NTC ceramic preform; Step 4, the NTC ceramic preform in step 3 is subjected to rapid sintering treatment, firstly the temperature is raised to 1100-1180°C and kept for 1-3h, then the temperature is raised to 1650-1680°C and kept for 1-3h, then the temperature is raised to 2180-2250°C and kept for 0.5-1h, and finally the temperature is lowered to 800-850°C, and the semi-finished NTC thermistor material is obtained after the furnace is opened and naturally cooled to room temperature; Step 5: De-stress the semi-finished NTC thermistor material obtained in step 4 by first heating it to 200-240°C and keeping it for 1-2 hours under an inert atmosphere, then heating it to 400-420°C at a rate of 40-80°C / min and keeping it for 4-8 hours, and finally opening the furnace and naturally cooling it to room temperature to obtain a finished high entropy oxide-based thermistor.
9. The method for preparing a thermistor based on high entropy oxide according to claim 8, characterized in that: In the step three, the obtained mixed powder is placed in a molding mold for cold isostatic pressing, the molding temperature is 20-50°C, and the molding pressure is: first pressurized to 200MPa at 10MPa / s, maintained for 60s, then pressurized to 360MPa at 5MPa / s, maintained for 180s, then reduced to 200MPa at 5MPa / s, maintained for 30s, and then reduced to 0MPa at 20MPa / s. The molding speed is 0.5mm / s. After completing the cold isostatic pressing process, the NTC ceramic preform can be obtained.