A corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitor and a preparation method thereof, and an electrolytic capacitor
By using electrolytes of aryl boric acid compounds in high-voltage aluminum electrolytic capacitors, using their electrophilicity and electron-absorbing properties to bind anions such as halogen, the corrosion problem of the capacitor in harsh environments is solved, and the corrosion resistance of the capacitor is significantly improved and lifespan.
Patent Information
- Application Number
- CN202411162272.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Existing high-voltage aluminum electrolytic capacitors are susceptible to corrosion by halogen and sulfur in harsh environments, resulting in early failure. The existing electrolytes are insufficient corrosion resistance under high pressure conditions, especially for metal aluminum and oxide films under high chloride ion concentration. All have corrosion effects.
An electrolyte containing aryl boric acid compounds is used to increase the binding effect on anions such as halogen through the empty p orbital of boron atoms and the electron-absorbing properties of aryl groups, reduce its reaction rate with metals, and improve the corrosion resistance of the capacitor.
It effectively reduces the risk of corrosion failure of the capacitor in high voltage and high chloride ion environments, extends the life of the capacitor, and maintains good durability especially under high temperature load conditions of 105℃.
Smart Images

Figure SMS_1 
Figure SMS_7 
Figure SMS_8
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolyte for aluminum electrolytic capacitors, and in particular to a corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors and a preparation method thereof, and an electrolytic capacitor. Background Art
[0002] With the development of the power electronics field, the application scenarios of capacitors are becoming more and more complex. For example, on-board OBC, outdoor power supply, outdoor photovoltaic, wind power and other equipment inevitably work in relatively harsh environments. In these harsh environments, substances containing halogens (Cl, Br), sulfur and other substances penetrate into the capacitor from the sealing edge of the capacitor, pressure valve and other locations in the form of gas, causing early corrosion failure of the capacitor. The rate of corrosion failure is related to factors such as halogen / sulfur ion concentration, working voltage, and working temperature. For high-voltage capacitors of 350V~550V, the corrosion reaction rate is particularly sensitive to chloride ion concentration. He Xiaoyun of Jianghai Capacitor and Huang Xinggao of ZTE Corporation jointly found that in the 450V high-voltage capacitor used in UPS, the chloride ion concentration reached 5ppm, and the anode corrosion open circuit failure occurred after working at the rated voltage of 105℃ for 500h. In these harsh environments, higher requirements are placed on the corrosion resistance of high-voltage capacitors.
[0003] Chinese patent CN10752774 B discloses an electrolyte for low-corrosive electrolytic capacitors and a preparation method thereof, using a corrosion inhibitor composed of 8-hydroxyquinoline and silicon dioxide. 8-Hydroxyquinoline can react with Al 3+ The formation of complexes, but the amount of complexes will affect the flash voltage of the electrolyte; secondly, the colloidal particles containing silicon dioxide may condense and precipitate in the electrolyte, which will eventually lead to a decrease in the withstand voltage of the electrolyte. This electrolyte is mainly suitable for medium and low voltage specifications within a rated voltage of 160V, and is limited in use in high-voltage products.
[0004] Chinese patent CN107845504B discloses an electrolyte with excellent anti-corrosion performance, which uses organic polysilicic acid compounds as corrosion inhibitors. In 450V~500V aluminum electrolytic capacitors, after adding 5ppm chloride ions, the load life at 105℃ is 5000 hours. In most cases, the chloride ion concentration of the raw materials inside the capacitor can be guaranteed to be within 5ppm. When encountering a harsh environment and external harmful substances invading, the chloride ions inside the capacitor will rise to a higher level, and most electrolytes still have a high corrosion risk to the capacitor.
[0005] Chinese patent CN113593908A discloses a nitrogen-containing amine or amide corrosion inhibitor, which changes the charge state and interface properties of the metal surface through the adsorption of polar groups in the corrosion inhibitor molecules, thereby slowing down the corrosion rate of the metal. However, for high-voltage capacitors, there is a relatively dense oxide film Al2O3 on the surface of the aluminum foil, which itself protects the metal aluminum inside. However, in the presence of high concentrations of chloride ions, in addition to corroding the metal aluminum, the oxide film Al2O3 on the surface is also strongly corrosive, and the anti-corrosion effect of this type of corrosion inhibitor is limited. Summary of the invention
[0006] In order to solve the problem of insufficient working life of capacitors under high halogen concentration conditions in the prior art, a corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors and a preparation method thereof, and an electrolytic capacitor are provided. The electrolyte of the present invention is used in high-voltage aluminum electrolytic capacitors to effectively reduce the risk of capacitor corrosion failure.
[0007] In order to achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A corrosion-resistant electrolyte for a high-voltage aluminum electrolytic capacitor comprises the following components: a solvent, a solute, an additive and an aromatic boronic acid compound, wherein the aromatic boronic acid compound has any one of the following chemical structures:
[0009]
[0010] The R substituent is selected from a nitro group, a fluorinated alkyl group, a carboxyl group, a hydroxyl group, an alkoxy group, and an alkyl ester group.
[0011] Preferably, the R substituent is selected from the following groups: NO2, CF3, COOH, OH; the R substituent in chemical structure I and chemical structure III is at the 3rd or 4th position relative to the boron atom, and the R substituent in chemical structure II and chemical structure IV forms a homobenzene structure with the boron atom in a single benzene ring.
[0012] More preferably, the arylboronic acid compound is selected from any one or more of the following chemical structures:
[0013] , , , , .
[0014] Furthermore, the electrolyte includes the following components in percentage by mass: 65%-75% solvent, 8%-18% solute, 9%-15% additive, and 1%-12% aromatic boronic acid compound.
[0015] Furthermore, the solvent is selected from one or more of ethylene glycol, diethylene glycol, and propylene glycol; the solute is selected from one or more of ammonium pentaborate, ammonium azelaic acid, ammonium sebacate, and 1,6-dodecanedioic acid; and the additive is selected from one or more of a flash enhancer, an anti-hydration agent, and a hydrogen absorber.
[0016] Preferably, the electrolyte comprises the following components in percentage by mass: main solvent 50%-70%, auxiliary solvent 3%-15%, solute 8%-18%, flash enhancer 7%-12%, anti-hydration agent 0.3%-4%, hydrogen absorber 0.5%-1.5%, and aromatic boric acid compound 1%-12%.
[0017] Preferably, the alcohol solvent is a combination of ethylene glycol and diethylene glycol or glycerol, wherein the ethylene glycol is used as the main solvent, the main solvent is ethylene glycol, and the auxiliary solvent is diethylene glycol or glycerol;
[0018] The flash enhancer is selected from one or more of PEG, PVA, and nano-silica; the anti-hydration agent is selected from one or more of ammonium dihydrogen phosphate, mannitol, and aluminum silicate; the hydrogen absorber is selected from one or more of p-nitrobenzyl alcohol, m-nitroacetophenone, o-nitroanisole, and p-nitrophenol.
[0019] Another aspect of the present invention provides a method for preparing the corrosion-resistant electrolyte for the high-voltage aluminum electrolytic capacitor, comprising the following steps:
[0020] S1, heating the solvent to a first temperature, adding the solute and heating it to a second temperature, stirring and dissolving evenly;
[0021] S2, adding additives: flash enhancer and anti-hydration agent, continuing to heat up to the third temperature, stirring and dissolving evenly, and then cooling down to the fourth temperature;
[0022] S3, adding an aromatic boric acid compound and an additive hydrogen absorber at the fourth temperature, heating to a fifth temperature and boiling for no more than 2 hours, and naturally cooling to obtain a corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors.
[0023] Furthermore, the first temperature is 60°C-100°C, the second temperature is 100°C-120°C, the third temperature is 110°C-135°C, the fourth temperature is 85°C-95°C, the fifth temperature is 90°C-110°C, and the cooking time is 30min-120min.
[0024] A third aspect of the present invention provides an electrolytic capacitor, wherein the electrolytic capacitor includes the above-mentioned corrosion-resistant electrolyte for a high-voltage aluminum electrolytic capacitor.
[0025] Furthermore, the electrolytic capacitor also includes an element formed by an anode foil, a cathode foil and an electrolytic paper, the electrolytic paper is arranged between the anode foil and the cathode foil, and the electrolytic paper is soaked with the electrolyte; the electrolytic capacitor is selected from one of a solid electrolytic capacitor, a liquid electrolytic capacitor, and a solid-liquid hybrid electrolytic capacitor.
[0026] Furthermore, the electrolytic capacitor is a liquid aluminum electrolytic capacitor, the element is immersed in the electrolyte, and the electrolytic capacitor also includes a metal shell for accommodating the element and the electrolyte and a sealing member for sealing the metal shell.
[0027] Beneficial technical effect: The present invention adds a small amount of aromatic boric acid compounds to the electrolyte of high-voltage aluminum electrolytic capacitors to effectively reduce the risk of capacitor corrosion failure. This is because the boron atom contains an empty p orbital, which can accept electrons and has certain electrophilic properties. Due to the electron-withdrawing properties of the aromatic group, the electrophilicity of the p orbital of the boron atom is enhanced. Therefore, in the presence of anions such as halogens and sulfur elements, the p orbital of the boron atom has a strong binding effect on anions such as halogens, limits the activity of anions such as halogens, and greatly reduces the reaction rate of anions such as halogens with Al or Al2O3, thereby reducing the risk of capacitor corrosion failure; the aromatic boric acid compounds with electron-withdrawing substituents in the present invention are used in the electrolyte, compared with the aromatic boric acid compounds with electron-donating substituents, and have better corrosion resistance for high-voltage aluminum electrolytic capacitors in high chloride ion concentrations. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0030] In addition, it should be noted that the use of words such as "first" and "second" to express temperature is only to facilitate the distinction between the temperatures involved in each step. Unless otherwise stated, the above words have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0031] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.
[0032] The information of the aryl boronic acid compounds used below is shown in Table 1 below.
[0033] Table 1 Information on arylboronic acid compounds
[0034]
[0035] Compound 4 is publicly known, see: Guan Changwei. Synthesis and Application Research of Arylboronic Acid Compounds [D]. East China University of Science and Technology, 2018, P29.
[0036] Compound 5 is publicly known, see: Lai, Yu-Ying, Bornand, Marc, Chen, Peter. Homogeneous model complexes for supported rhenia metathesis catalysts [J]. Organometallics 2013, P7558-7565.
[0037] Example 1
[0038] A corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors, comprising the following components in percentage by weight: 73 wt% of an alcohol solvent, 8 wt% of a solute, 9 wt% of an additive, and 10 wt% of an aromatic boronic acid compound (compound 1);
[0039] Among them, the main solvent of the alcohol solvent is ethylene glycol, which accounts for 65wt% of the electrolyte, and the auxiliary solvent is diethylene glycol, which accounts for 8wt% of the electrolyte;
[0040] Among them, the solutes are 1,6-dodecanedioic acid ammonium, ammonium pentaborate, and ammonium azelaic acid, which account for 4wt%, 2wt%, and 2wt% in the electrolyte respectively;
[0041] Among them, the additives are flash enhancer, anti-hydration agent and hydrogen absorber; the flash enhancer is composed of PVA-105 and nano-silica, PVA-105 accounts for 1.5wt% in the electrolyte, and nano-silica accounts for 6wt% in the electrolyte; the anti-hydration agent is ammonium dihydrogen phosphate, accounting for 0.5wt% in the electrolyte; the hydrogen absorber is m-nitroacetophenone, accounting for 1wt% in the electrolyte.
[0042] The preparation method of the above electrolyte comprises the following steps:
[0043] S1, heating the solvent to a first temperature of 80°C, adding the solute and heating it to a second temperature of 110°C, stirring and dissolving evenly;
[0044] S2, adding additives: flash enhancer and anti-hydration agent, continuing to heat up to the third temperature of 120°C, stirring and dissolving evenly, and then cooling down to the fourth temperature of 90°C;
[0045] S3, adding an aromatic boric acid compound and an additive hydrogen absorber at the fourth temperature, heating to a fifth temperature of 100° C. and boiling for 60 minutes, and naturally cooling to obtain a corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors.
[0046] The above specific materials used and their proportions are shown in Table 2.
[0047] Example 2
[0048] The electrolyte composition ratio of Example 2 is shown in Table 2. The electrolyte preparation method of Example 2 comprises the following steps:
[0049] S1, heating the solvent to a first temperature of 65°C, adding the solute and heating it to a second temperature of 100°C, stirring and dissolving evenly;
[0050] S2, adding additives: flash enhancer and anti-hydration agent, continuing to heat up to the third temperature of 110°C, stirring and dissolving evenly, and then cooling down to the fourth temperature of 95°C;
[0051] S3, adding an aromatic boric acid compound and an additive hydrogen absorber at the fourth temperature, heating to a fifth temperature of 110° C. and boiling for 35 minutes, and naturally cooling to obtain a corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors.
[0052] Example 3
[0053] The electrolyte composition ratio of Example 3 is shown in Table 2. The electrolyte preparation method of the embodiment comprises the following steps:
[0054] S1, heating the solvent to a first temperature of 100°C, adding the solute and heating it to a second temperature of 120°C, stirring and dissolving evenly;
[0055] S2, adding additives: flash enhancer and anti-hydration agent, continuing to heat up to the third temperature of 130°C, stirring and dissolving evenly, and then cooling down to the fourth temperature of 85°C;
[0056] S3, adding an aromatic boric acid compound and an additive hydrogen absorber at the fourth temperature, heating to a fifth temperature of 90° C. and boiling for 100 minutes, and naturally cooling to obtain a corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors.
[0057] Example 4-Example 6
[0058] The electrolyte composition ratios of Examples 4 to 6 are shown in Table 2. The electrolyte preparation methods of Examples 4 to 6 are the same as those of Example 1.
[0059] Comparative Example 1-Comparative Example 3
[0060] The electrolyte composition ratios of Comparative Examples 1 to 3 are shown in Table 2.
[0061] The electrolyte in Table 2 is calculated based on 100% mass percentage, and the unit of the values in Table 2 is wt%.
[0062] Table 2 Electrolyte composition ratios for each case
[0063]
[0064] (Note: “ / ” means not added)
[0065] Test Example 1
[0066] Chloride ions with a mass percentage concentration of 5ppm, 10ppm, and 20ppm were added to the electrolytes of the above cases respectively under initial conditions, and the flash voltage of the electrolytes of each case was tested after stirring evenly. The specific results are shown in Table 3 below.
[0067] Table 3 Flash voltage after adding chloride ions to the electrolyte of each case
[0068]
[0069] (Note: The unit of each value in the table is V)
[0070] As can be seen from Table 3, the electron-withdrawing groups NO2, CF3, and COOH in the aromatic boric acid compounds can increase the resistance of the electrolyte to chloride ions. When the chloride ion concentration of Examples 1-6 reaches 20 ppm, the flash voltage of the electrolyte can still be maintained above 490 V.
[0071] Although an aromatic boronic acid compound is also used in Comparative Example 1, the hydroxyl group in Compound 6 is an electron-donating group, the acidity of the aromatic boronic acid is weakened, and the binding force to anions is reduced. When the chloride ion content in the electrolyte is 10ppm, the electrolyte flash voltage can be maintained above 490V, but when the chloride ion content in the electrolyte is 20ppm, the flash voltage can only be maintained above 450V.
[0072] Comparative Examples 2 and 3 did not add aromatic boric acid compounds. When 5 ppm of chloride ions were added to the electrolyte, the flash voltage dropped significantly by more than 50 V. As the chloride ion concentration increased to 20 ppm, the flash voltage of the electrolyte dropped sharply to less than 300 V.
[0073] Based on the stability of the flash voltage of the electrolyte in different chloride ion concentrations, the corrosion resistance of the electrolyte can be preliminarily judged: when a certain concentration of chloride ions is added, the lower the flash voltage of the electrolyte decreases compared to the initial value, the stronger its corrosion resistance is.
[0074] In order to further illustrate the corrosion resistance of the electrolyte of the present invention, the electrolytes of Examples 1 to 6 and Comparative Examples 1 to 3 were used as working electrolytes for capacitors.
[0075] The preparation of aluminum electrolytic capacitors includes the following steps: the element is wound with anode foil, cathode foil, electrolytic paper, and lead wire, and the element is immersed in the electrolyte of Examples 1 to 6 and Comparative Examples 1 to 3 respectively, and the impregnated element is continuously sealed with an aluminum shell and a cover plate, and a high-voltage aluminum electrolytic capacitor is obtained after aging. At the same time, the same capacitor is made according to the above process, except that 5ppm, 10ppm, and 20ppm of chloride ions are added to the electrolyte respectively. The capacitor manufacturing specifications are: 450V470μF, size D35mm×L45mm.
[0076] The capacitors prepared above were subjected to a 105°C high temperature load life test experiment, and 10 capacitors were tested in each group of embodiments. High temperature load test conditions: temperature 105°C, frequency 120Hz, ripple current 2.0A / pcs, voltage is rated voltage.
[0077] The durability test results are shown in Tables 4 to 6.
[0078] Table 4 Adding 5ppm chloride ions
[0079]
[0080] Table 5 Adding 10ppm chloride ions
[0081]
[0082] Table 6 Addition of 20ppm chloride ions
[0083]
[0084] As shown in Table 4, when the electrolyte was added with 5ppm chloride ions, Examples 1-6 added aryl boric acid compounds (Compounds 1-Compound 5) with electron-withdrawing substituents. The benzene rings of these compounds were connected with electron-withdrawing groups, which had strong binding force on chloride ions and passed the 105°C 5000h durability test. After the test, the capacitor was disassembled and no corrosion failure was found. Comparative Example 1 added aryl boric acid compounds (Compound 6) with electron-donating substituents. The benzene ring of Compound 6 was connected with hydroxyl groups of electron-donating groups, which weakened the binding force on chloride ions. The capacitance Lc began to increase at 3000h of the durability test. When the test reached 4000h, one capacitor had no capacity. When the test reached 5000h, a total of 2 capacitors were corroded. Comparative Examples 2 and 3 had 10% and 20% corrosion failures at 1000h and 2000h, respectively. The corrosion ratio reached more than 50% at 3000h, and the test was stopped.
[0085] Table 5 shows the test results of adding 10ppm chloride ions to the electrolyte. Examples 1-6 all passed the durability test at 105℃ for 5000h. The capacitance Lc of Comparative Example 1 began to increase after 2000h. After 3000h, one capacitor had no capacity. Dissection revealed that the anode lead wire was corroded and broken, and the circuit was open. As the test time increased, the corrosion ratio of Comparative Example 1 continued to increase. After 5000h, the corrosion failure rate reached 60%. Comparative Examples 2 and 3 had 50% and 40% corrosion failures at 1000h, respectively, and the experiment was stopped immediately.
[0086] Table 6 shows the test results of adding 20ppm chloride ions to the electrolyte. Examples 1 to 6 all passed the 105℃ 5000h durability assessment. Comparative Example 1 began to increase the capacitance Lc after 1000h of the test. After 2000h of the test, two capacitors had no capacity. Dissection revealed that the anode lead wire was corroded and broken, and the circuit was open. As the test time increased, the corrosion ratio of Comparative Example 1 continued to increase. After 5000h of the test, the corrosion open circuit failure rate reached 90%. Comparative Examples 2 and 3 corroded during the preparation and aging stage, and no experiments were performed.
[0087] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors, characterized in that: The invention comprises the following components: a solvent, a solute, an additive and an aromatic boronic acid compound, wherein the aromatic boronic acid compound has any one of the following chemical structures: The R substituent is selected from the following groups: NO2, CF3, COOH; the R substituent in chemical structure I and chemical structure III is at the 3rd or 4th position relative to the boron atom, and the R substituent in chemical structure II and chemical structure IV forms a homobenzene structure with the boron atom in a single benzene ring; The preparation method of the corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors comprises the following steps: S1, heating the solvent to a first temperature, adding the solute and heating it to a second temperature, stirring and dissolving evenly; S2, adding additives: flash enhancer and anti-hydration agent, continuing to heat up to the third temperature, stirring and dissolving evenly, and then cooling down to the fourth temperature; S3, adding an aromatic boric acid compound and an additive hydrogen absorber at the fourth temperature, heating to a fifth temperature and boiling for no more than 2 hours, and naturally cooling to obtain a corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors; The first temperature is 60°C-100°C, the second temperature is 100°C-120°C, the third temperature is 110°C-135°C, the fourth temperature is 85°C-95°C, and the fifth temperature is 90°C-110°C.
2. The corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitor according to claim 1, characterized in that: The aromatic boronic acid compound is selected from any one or more of the following chemical structures:
3. A corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitors according to any one of claims 1 to 2, characterized in that: The electrolyte comprises the following components in percentage by weight: 65%-75% solvent, 8%-18% solute, 9%-15% additive, and 1%-12% arylboronic acid compound; The solvent is selected from one or more of ethylene glycol, diethylene glycol, and glycerol; The solute is selected from one or more of ammonium pentaborate, ammonium azelaic acid, ammonium sebacate, and 1,6-dodecanedioic acid.
4. The corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitor according to claim 3, characterized in that: The electrolyte comprises the following components in percentage by mass: 50%-70% of a main solvent, 3%-15% of an auxiliary solvent, 8%-18% of a solute, 7%-12% of a flash enhancer, 0.3%-4% of an anti-hydration agent, 0.5%-1.5% of a hydrogen absorber, and 1%-12% of an aromatic boric acid compound.
5. The corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitor according to claim 4, characterized in that: The main solvent is ethylene glycol, and the auxiliary solvent is diethylene glycol or glycerol; The flash enhancement agent is selected from one or more of PEG, PVA, and nano-silicon dioxide; The anti-hydration agent is selected from one or more of diammonium phosphate, mannitol, and aluminum silicate; The hydrogen absorbent is selected from one or more of p-nitrobenzyl alcohol, m-nitroacetophenone, o-nitroanisole and p-nitrophenol.
6. The corrosion-resistant electrolyte for high-voltage aluminum electrolytic capacitor according to claim 1, characterized in that: The cooking time is 30 min-120 min.
7. An electrolytic capacitor, characterized in that: The electrolytic capacitor comprises a corrosion-resistant electrolyte for a high-voltage aluminum electrolytic capacitor as described in any one of claims 1 to 6.
8. An electrolytic capacitor according to claim 7, characterized in that: The electrolytic capacitor further includes an element formed by an anode foil, a cathode foil and electrolytic paper. The electrolytic paper is arranged between the anode foil and the cathode foil, and the electrolytic solution is impregnated on the electrolytic paper.