An industrial application perovskite solar cell module and preparation method thereof
By using alloyed tellurium oxide as hole transport material and vacuum thermal evaporation deposition method in perovskite solar cell modules, the problems of low efficiency and high cost in large-area applications of perovskite solar cell modules are solved, and the problem of low efficiency and high cost is achieved. High performance, high stability and low cost industrial production.
Patent Information
- Application Number
- CN202411163682.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing perovskite solar cell modules are inefficient in large-area applications, and traditional hole transport materials are costly and have poor stability, making them difficult to be suitable for industrial production.
The perovskite solar cell module is prepared by vacuum thermal evaporation deposition method, including etching the transparent electrode layer to form trenches, deposition of hole transport layer, perovskite light-absorbing layer and electron transport The metal electrode layer is formed by laser etching to achieve efficient charge transport and stability.
It improves the charge transfer capability and stability of perovskite solar cell modules, reduces production costs, is suitable for large-scale industrial production, and realizes high-performance and high-stability perovskite solar cell modules.
Smart Images

Figure CN118678847B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photovoltaic devices, and specifically relates to an industrially applicable perovskite solar cell module and a preparation method thereof. Background Art
[0002] Perovskite materials have attracted extensive attention in the field of optoelectronic devices such as solar cells, photodiodes, memristors, and phototransistors due to their excellent optoelectronic properties. Among them, perovskite solar cell devices have the advantages of high energy conversion efficiency, low process equipment cost, simple preparation process, and solution preparation, becoming a new research hotspot in the field of solar cells. After just over a decade of development, the energy conversion efficiency of perovskite solar cells has rapidly increased from the initial 3.8% to 26.1%, which is comparable to single-crystal silicon cells. However, the excellent optoelectronic performance is only manifested in small-area devices, and the efficiency of large-area modules is much lower than the former. At the same time, the preparation method of small-area high-efficiency devices is mainly achieved by solution spin coating, which is not suitable for large areas. Therefore, the research on perovskite solar cell modules is an important part of its commercial development process. As a light absorption layer, the film quality and transmission performance of the perovskite film determine the quality of the battery device. The hole transport layer, which is also a functional layer, is an important component of the perovskite solar cell. Its main function is to block electrons, collect holes injected by the perovskite light absorption layer and transmit them to the metal electrode to achieve effective separation of electrons and holes. Its hole transport performance is one of the key factors that determine the performance of perovskite solar photovoltaics. At the same time, the hole transport layer also plays a leading role in device performance and long-term stability. In the pin-type device structure, the hole transport material should have a suitable band structure, high carrier mobility, and good light and heat resistance.
[0003] At present, the mainstream hole transport materials used in trans-perovskite solar cell modules are P3HT, PTAA, PEDOT:PSS, NiO X and Spiro-TTB, etc. Conjugated polymer hole transport materials such as P3HT, PTAA and PEDOT:PSS have complicated synthesis routes and difficult purification steps, resulting in high material costs. Moreover, they are organic materials with poor stability. In addition, these materials are generally prepared by spin coating, which produces large-area thin films with poor uniformity and high defect density, thus affecting device performance and making them unsuitable for industrial production. NiO x As an oxide hole transport material, NiO has better conductivity and film stability than organic polymer materials. xThin films are generally prepared by solution method and magnetron sputtering method. The uniformity and crystallization of large-area thin films prepared by solution method are poor, which is not suitable for large-scale industrial production. At the same time, the purchase and maintenance costs of magnetron sputtering equipment are very high, resulting in high industrialization costs. At present, low-cost industrial preparation processes mostly use vacuum thermal evaporation deposition, which has a simple process, low cost, and good repeatability. Spiro-TTB hole transport layer is commonly prepared by vacuum thermal evaporation deposition. The thin film prepared by this method has good uniformity and few defects, but Spiro-TTB material, as an organic material, is very sensitive to environmental factors such as water vapor, temperature and light, resulting in poor stability of perovskite solar cells; in addition, the synthesis and purification process of this material is very complicated, the production cost is high, and the scope of application is limited. Therefore, how to realize low-cost perovskite solar cell module technology that can be industrialized is urgently needed. Summary of the invention
[0004] In order to solve the above problems existing in the prior art, the present invention provides an industrial application perovskite solar cell module and a preparation method thereof. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0005] The embodiment of the present invention provides a method for preparing a perovskite solar cell module for industrial application, comprising the steps of:
[0006] S1, etching the transparent electrode layer to form a plurality of first grooves, wherein the plurality of first grooves divide the transparent electrode layer into a plurality of sub-cell regions;
[0007] S2. Depositing a hole transport material on the surface of the plurality of sub-cell regions and in the plurality of first grooves to form a hole transport layer; wherein the material of the hole transport layer comprises alloyed tellurium oxide, and the alloyed tellurium oxide is formed by mixing tellurium oxide with any one alloy element selected from the group consisting of Se, S, P, As, Mg, Fe, and Al;
[0008] S3, depositing a perovskite light absorbing layer on the surface of the hole transport layer;
[0009] S4, depositing an electron transport layer on the surface of the perovskite light absorbing layer;
[0010] S5, etching the electron transport layer, the perovskite light absorption layer and the hole transport layer until the transparent electrode layer, exposing a portion of the surface of the first end sub-cell region and a portion of the surface of the second end sub-cell region in the plurality of sub-cell regions, and forming a second groove above the middle sub-cell region of the plurality of sub-cell regions;
[0011] S6, depositing a metal electrode layer, wherein one end of the metal electrode layer extends from the surface of the electron transport layer to the surface of the first end sub-battery region, and the other end of the metal electrode layer extends from the surface of the electron transport layer to the surface of the second end sub-battery region, and is filled in the second groove;
[0012] S7. Etch the metal electrode layer of the first end sub-cell region until the transparent electrode layer, so that the metal electrode layer on the surface of the first end sub-cell region is at a preset distance from the hole transport layer, and at the same time, etch the metal electrode layer, electron transport layer, perovskite light absorption layer and hole transport layer above each intermediate sub-cell region until the transparent electrode layer to form a third groove, to obtain a plurality of sub-cells interconnected by the metal electrode layer in the second groove.
[0013] In one embodiment of the present invention, step S1 comprises:
[0014] Laser etching the transparent electrode layer, with an etching depth greater than or equal to the thickness of the transparent electrode layer, to form the plurality of first grooves; wherein the laser frequency is 300-500 kHz, the etching speed is 1800-2200 mm / s, the etching times is 2 times, and the laser wavelength is 1064 nm;
[0015] The transparent electrode layer is cleaned.
[0016] In one embodiment of the present invention, in the alloyed tellurium oxide, the mass of tellurium oxide is 280-320 mg, and the mass of the alloy element is 8-24 mg.
[0017] In one embodiment of the present invention, step S2 comprises:
[0018] Using vacuum thermal evaporation deposition method, the vacuum pressure is 3×10 -4 -5×10 -4 At a evaporation rate of 0.4-0.6 Å / s, depositing 70-90 nm of hole transport material on the surfaces of the plurality of sub-cell regions and in the plurality of first grooves to form a hole transport layer;
[0019] The hole transport layer is annealed in air at a temperature of 150-250° C. for 20-40 minutes.
[0020] In one embodiment of the present invention, the general structural formula of the perovskite light absorbing layer material is ABX3, wherein A is a cation and A is selected from MA + , FA + , Rb + , Cs + One or more of; B is a cation and B is selected from Pb 2+ Sn2+ One or more of; C is an anion and is selected from Cl - Br - ,I - One or more of;
[0021] When the perovskite light absorbing layer is Cs 0.05 FA 0.70 MA 0.25 PbI 2.75 Br 0.25 When , step S3 includes:
[0022] Using vacuum thermal evaporation deposition method, at a pressure of 3×10 -4 -5×10 -4 Pa, deposit PbI2 and CsI with a total thickness of 310-350nm on the surface of the hole transport layer at a evaporation rate of 0.8-1.2Å / s; then deposit 210-250nm of FAI at a evaporation rate of 0.8-1.2Å / s; finally deposit 30-50nm of MABr at a evaporation rate of 0.4-0.6Å / s; and anneal in an air environment at 110-130℃ for 15-30min to obtain a Cs 0.05 FA 0.70 MA 0.25 PbI 2.75 Br 0.25 Perovskite light-absorbing layer.
[0023] In one embodiment of the present invention, step S4 includes:
[0024] Using vacuum thermal evaporation deposition method, at a pressure of 3×10 -4 -5×10 -4 Pa, under the condition of an evaporation rate of 0.4-0.6Å / s, 20-40nm of electron transport material is deposited on the surface of the perovskite light absorbing layer, and then under the condition of an evaporation rate of 0.1-0.2Å / s, 5-10nm of interface modification material is deposited to form the electron transport layer.
[0025] In one embodiment of the present invention, step S5 includes:
[0026] Laser etching the electron transport layer, the perovskite light absorption layer and the hole transport layer until the transparent electrode layer, exposing a portion of the surface of the first end sub-cell region and a portion of the surface of the second end sub-cell region in the plurality of sub-cell regions, and forming a second groove above the middle sub-cell region of the plurality of sub-cell regions;
[0027] Among them, the laser frequency is 800-1200kHz, the etching speed is 600-1000mm / s, the etching number is 1 time, and the laser wavelength is 355nm.
[0028] In one embodiment of the present invention, step S6 includes:
[0029] Using vacuum thermal evaporation deposition method, at a pressure of 3×10 -4 -5×10 -4 Pa, and a 130-160nm metal electrode layer was deposited at an evaporation rate of 0.6-1.0Å / s.
[0030] In one embodiment of the present invention, step S7 includes:
[0031] Laser etching the metal electrode layer of the first end sub-cell region to the transparent electrode layer, so that the metal electrode layer on the surface of the first end sub-cell region is at a preset distance from the hole transport layer, and laser etching the metal electrode layer, the electron transport layer, the perovskite light absorption layer and the hole transport layer above each intermediate sub-cell region to the transparent electrode layer to form a third groove, thereby obtaining a plurality of sub-cells interconnected by the metal electrode layer in the second groove;
[0032] Among them, the laser frequency is 400-800kHz, the etching speed is 2200-2600mm / s, the etching number is 1 time, and the laser wavelength is 355nm.
[0033] Another embodiment of the present invention provides an industrialized perovskite solar cell module, which is prepared by the preparation method described in the above embodiment, and includes: a substrate, a transparent electrode layer, a hole transport layer, a perovskite light absorption layer, an electron transport layer and a metal electrode layer, wherein the transparent electrode layer is located on the substrate, and a plurality of first grooves are formed in the transparent electrode layer, and the plurality of first grooves divide the transparent electrode layer into a plurality of sub-cell regions;
[0034] The hole transport layer is located on the surface of the middle sub-cell region among the plurality of sub-cell regions, part of the surface of the first end sub-cell region and part of the surface of the second end sub-cell region, and is filled in the plurality of first grooves; the material of the hole transport layer is alloyed tellurium oxide, and the alloyed tellurium oxide is formed by mixing tellurium oxide with any one alloy element of Se, S, P, As, Mg, Fe, and Al;
[0035] The perovskite light absorption layer and the electron transport layer are sequentially stacked on the surface of the hole transport layer; a second groove is formed above each of the intermediate sub-cell regions, and the second groove runs through the electron transport layer, the perovskite light absorption layer and the hole transport layer;
[0036] The metal electrode layer fills a plurality of the second grooves and extends from the surface of the electron transport layer to the surface of the second end sub-battery region; the metal electrode layer located on the surface of the first end sub-battery region is at a preset distance from the hole transport layer;
[0037] A third groove is formed above each of the intermediate sub-cell regions, and the third groove penetrates the metal electrode layer, the electron transport layer, the perovskite light absorption layer and the hole transport layer to form a plurality of sub-cells interconnected by the metal electrode layer in the second groove.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1. The material of the hole transport layer of the present invention adopts any one of Se, S, P, As, Mg, Fe, Al alloy elements and tellurium oxide to form alloyed tellurium oxide; first, the alloyed tellurium oxide has high mobility, which can effectively improve the charge transfer capacity of the perovskite solar cell module, thereby improving the efficiency of the large-area perovskite solar cell module; second, the alloyed tellurium oxide is an oxide material, which is insensitive to air oxidation and has good air stability and thermal stability; third, the raw material price of alloyed tellurium oxide is low, the cost is low, and it is suitable for large-scale production by vacuum thermal evaporation deposition method; therefore, the present invention adopts alloyed tellurium oxide as the hole transport layer, which can realize a high-performance, high-stability and low-cost perovskite solar cell module.
[0040] 2. The hole transport layer, perovskite light absorption layer, electron transport layer and metal electrode layer of the present invention are all prepared by vacuum thermal evaporation deposition method, which is suitable for the preparation of large-area highly repeatable perovskite solar cell modules; first, in the vacuum thermal evaporation deposition method, the film is prepared under vacuum conditions, has excellent film uniformity, avoids contamination by impurities and gases, and is conducive to the high performance and high stability of the film and the device; second, the preparation process can accurately control the film thickness, has high controllability and repeatability, does not contain toxic solvents, and has excellent device reproducibility and scalability, which is suitable for the preparation of large-area module devices, and significantly improves the high yield rate of industrial applications of perovskite solar cell modules; third, compared with other deposition technologies, the structure of the vacuum thermal evaporation deposition equipment is relatively simple and the maintenance cost is low; therefore, the present invention realizes the preparation of perovskite solar cell modules by full vacuum thermal evaporation deposition method, which is conducive to the industrial development of perovskite solar cell modules. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 A schematic diagram of a process for preparing a perovskite solar cell module for industrial application provided by an embodiment of the present invention;
[0042] Figure 2a-2hA schematic diagram of a process for preparing a perovskite solar cell module for industrial application provided by an embodiment of the present invention;
[0043] Figure 3 A top view of an industrially applicable perovskite solar cell module provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0044] The present invention is further described in detail below with reference to specific embodiments, but the embodiments of the present invention are not limited thereto.
[0045] Embodiment 1
[0046] See also Figure 1 and Figure 2a-2h , Figure 1 A schematic diagram of a process for preparing a perovskite solar cell module for industrial application provided by an embodiment of the present invention, Figure 2a-2h A schematic diagram of a process for preparing a perovskite solar cell module for industrial application provided in an embodiment of the present invention.
[0047] The method for preparing the industrial application perovskite solar cell module comprises the following steps:
[0048] S1, etching the transparent electrode layer 1 to form a plurality of first grooves p1, wherein the plurality of first grooves p1 divide the transparent electrode layer 1 into a plurality of sub-cell regions, such as Figure 2a and Figure 2b shown.
[0049] First, the transparent electrode layer 1 is etched by laser, and the etching depth is greater than or equal to the thickness of the transparent electrode layer 1 to form a plurality of first grooves p1, so as to divide a plurality of sub-cell regions, and the two end regions of the plurality of sub-cell regions are respectively defined as the first end sub-cell region 111 and the second end sub-cell region 112, and each region between the two ends is defined as the middle sub-cell region 113. The conditions of laser etching are: the laser frequency is 300-500kHz, the etching speed is 1800-2200mm / s, the etching times is 2 times, and the laser wavelength is 1064nm. For example, the laser frequency is 400kHz, the etching speed is 2000mm / s, the etching times is 2 times, and the laser wavelength is 1064nm.
[0050] Specifically, the transparent electrode layer 1 can be made of any one of ITO and FTO, and the area can be 10×10 cm 2 .
[0051] Then, the transparent electrode layer 1 is cleaned.
[0052] Specifically, the sample is placed in Decon-90 cleaning agent, deionized water, acetone, alcohol and deionized water for ultrasonic cleaning, the ultrasonic cleaning temperature is 40-60°C, and the ultrasonic cleaning time of each solution is 20-40 minutes; after cleaning, it is blown dry with a nitrogen gun and placed in ultraviolet ozone for pretreatment, and the ultraviolet ozone pretreatment time is 20-40 minutes. Exemplarily, the ultrasonic cleaning temperature is 50°C, and the ultrasonic cleaning time of each solution is 30 minutes.
[0053] S2, depositing hole transport materials on the surfaces of several sub-cell regions and in several first grooves p1 to form a hole transport layer 2, such as Figure 2c shown.
[0054] Specifically, the hole transport layer 2 material includes alloyed tellurium oxide, and the alloyed tellurium oxide is formed by mixing any one of Se, S, P, As, Mg, Fe, and Al with tellurium oxide. Preferably, the alloyed tellurium oxide is formed by mixing Se and tellurium oxide. Compared with other alloy elements, using Se as an alloy element can achieve higher efficiency of the device.
[0055] Furthermore, in the alloyed tellurium oxide, the mass of tellurium oxide (TeO2) is 280-320 mg, and the mass of the alloying element is 8-24 mg.
[0056] Step S2 specifically includes:
[0057] First, a hole transport material is deposited on the surfaces of several sub-cell regions and in several first grooves p1 by using a vacuum thermal evaporation deposition method to form a hole transport layer 2 .
[0058] Specifically, the substrate obtained in step S1 is fixed on the substrate with a high temperature resistant tape, the hole transport material to be evaporated is placed in a crucible, the distance between the substrate baffle and the crucible is adjusted, and the vacuum pressure is evacuated to 3×10 -4 -5×10 -4 Pa. Then, the parameters of the vacuum thermal evaporation deposition instrument are set, and 70-90 nm of hole transport material is deposited at an evaporation rate of 0.4-0.6 Å / s to form a hole transport layer 2. Exemplarily, the evaporation rate is 0.5 Å / s, and the thickness of the hole transport layer 2 is 80 nm.
[0059] Then, the hole transport layer 2 is subjected to annealing treatment.
[0060] Specifically, after deposition, the vacuum thermal evaporation deposition instrument is turned off, and the substrate is taken out after the vacuum reaches atmospheric pressure. The hole transport layer is annealed in an annealing environment of air at an annealing temperature of 150-250° C. for 20-40 minutes. For example, the annealing time is 30 minutes, and the annealing temperature can be adjusted according to actual conditions.
[0061] S3, depositing a perovskite light absorbing layer 3 on the surface of the hole transport layer 2, such as Figure 2d shown.
[0062] Specifically, the general structural formula of the perovskite light absorbing layer 3 material is ABX3, wherein A is a cation and A is selected from MA + , FA + , Rb + , Cs + One or more of; B is a cation and B is selected from Pb 2+ Sn 2+ One or more of; C is an anion and is selected from Cl - Br - ,I - One or more of.
[0063] When the perovskite light absorbing layer 3 is made of Cs 0.05 FA 0.70 MA 0.25 PbI 2.75 Br 0.25 When , step S3 includes:
[0064] Using vacuum thermal evaporation deposition method, at a pressure of 3×10 -4 -5×10 -4 Pa, deposit PbI2 and CsI with a total thickness of 310-350nm on the surface of the hole transport layer 2 at a evaporation rate of 0.8-1.2Å / s; then deposit 210-250nm of FAI at a evaporation rate of 0.8-1.2Å / s; finally, deposit 30-50nm of MABr at a evaporation rate of 0.4-0.6Å / s; and anneal in an air environment at 110-130℃ for 15-30min to obtain a Cs 0.05 FA 0.70 MA 0.25 PbI 2.75 Br 0.25 Perovskite light absorbing layer 3.
[0065] For example, at a pressure of 5×10 -4 Pa, 230nm of FAI was deposited on the surface of the hole transport layer at a evaporation rate of 1.0Å / s; finally, 40nm of MABr was deposited at a evaporation rate of 0.5Å / s; and annealed in an air environment at 120°C for 20min to form a perovskite light absorbing layer 3.
[0066] S4, depositing an electron transport layer 4 on the surface of the perovskite light absorbing layer, such as Figure 2e shown.
[0067] Specifically, vacuum thermal evaporation deposition was performed at a pressure of 3×10 -4 -5×10 -4 Pa, a 20-40 nm electron transport material 41 is deposited on the surface of the perovskite light absorption layer at a evaporation rate of 0.4-0.6 Å / s, and then a 5-10 nm interface modification material 42 is deposited at a evaporation rate of 0.1-0.2 Å / s to form an electron transport layer 4. The electron transport material includes C 60 Or any one of PCBM, the interface modification material includes BCP.
[0068] For example, a vacuum thermal evaporation deposition method is used at a pressure of 5×10 -4 Pa, and a 30 nm C layer was deposited on the surface of the perovskite light absorbing layer at a evaporation rate of 0.5 Å / s. 60 Or PCBM, and then deposit 6nm of BCP at an evaporation rate of 0.1Å / s to form an electron transport layer 4.
[0069] S5, etching the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2 until the transparent electrode layer 1, exposing a portion of the surface of the first end sub-cell region 111 and a portion of the surface of the second end sub-cell region 112 in the plurality of sub-cell regions, and forming a second groove p2 above the middle sub-cell region 113 in the plurality of sub-cell regions, such as Figure 2f shown.
[0070] Specifically, the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2 are etched by laser until the transparent electrode layer 1 forms a second groove p2, and the etching depth is equal to the total thickness of the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2, so that the bottom transparent electrode layer 1 is exposed, and the interconnection position is reserved. Among them, the laser frequency is 800-1200kHz, the etching speed is 600-1000mm / s, the etching number is 1, and the laser wavelength is 355nm. Exemplarily, the laser frequency is 1000kHz, the etching speed is 800mm / s, the etching number is 1, and the laser wavelength is 355nm.
[0071] Furthermore, after laser etching, a portion of the surface outside the first end sub-cell region 111 and a portion of the surface outside the second end sub-cell region 112 are exposed, and a second trench p2 is formed above each middle sub-cell region 113 .
[0072] S6, depositing a metal electrode layer 5, wherein one end of the metal electrode layer 5 extends from the surface of the electron transport layer 4 to the surface of the first end sub-battery region 111, and the other end extends from the surface of the electron transport layer 4 to the surface of the second end sub-battery region 112, and is filled in the second groove p2, as shown in FIG. Figure 2g shown.
[0073] Specifically, vacuum thermal evaporation deposition was performed at a pressure of 3×10 -4 -5×10 -4 Pa, and a 130-160 nm metal electrode layer is deposited under the conditions of an evaporation rate of 0.6-1.0 Å / s. At this time, the metal electrode layer 5 covers the surface of the entire substrate, that is, the metal electrode layer 5 covers the surface of the electron transport layer 4, and covers the sides of the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2, and covers the surface of the first end sub-cell region 111 and the surface of the second end sub-cell region 112, and fills the second groove p2 at the same time. Exemplarily, a vacuum thermal evaporation deposition method is used at a pressure of 5×10 -4 Pa, and a 150nm metal electrode layer 5 was deposited at an evaporation rate of 0.8Å / s.
[0074] Specifically, the material of the metal electrode layer 5 includes any one of Ag, Cu, and Au.
[0075] S7, etching the metal electrode layer 5 of the first end sub-battery region 111 to the transparent electrode layer 1, so that the metal electrode layer 5 on the surface of the first end sub-battery region 111 is at a preset distance from the hole transport layer 2, and at the same time etching the metal electrode layer 5, the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2 above each intermediate sub-battery region 113 to the transparent electrode layer 1 to form a third groove p3, and obtain a plurality of sub-batteries interconnected by the metal electrode layer 5 in the second groove p2, such as Figure 2h shown.
[0076] Specifically, the metal electrode layer 5 of the first end sub-battery region 111 is etched by laser, and the etching depth is the thickness of the metal electrode layer 5, so that the metal electrode layer 5 on the surface of the first end sub-battery region 111 is at a preset distance from the hole transport layer 2, forming an independent metal electrode 6. At the same time, the metal electrode layer 5, the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2 above each intermediate sub-battery region 113 are etched by laser, and the transparent electrode layer 1 is exposed to form a third groove p3, and the etching depth is the total thickness of the metal electrode layer 5, the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2, so as to cut off the metal electrode layer 5, separate multiple sub-batteries, and make the sub-batteries interconnected only through the metal electrode layer 5 in the second groove p2.
[0077] Specifically, the laser frequency is 400-800kHz, the etching speed is 2200-2600mm / s, the etching times are 1 time, and the laser wavelength is 355nm. Exemplarily, the laser frequency of laser etching the third groove p3 is 600kHz, the etching speed is 2400mm / s, the etching times are 1 time, and the laser wavelength is 355nm.
[0078] In this embodiment, the material of the hole transport layer is formed by mixing any one of Se, S, P, As, Mg, Fe, and Al alloy elements with tellurium oxide to form alloyed tellurium oxide; first, the alloyed tellurium oxide has a high mobility, which can effectively improve the charge transfer capability of the perovskite solar cell module, thereby improving the efficiency of the large-area perovskite solar cell module; second, the alloyed tellurium oxide is an oxide material, which is insensitive to air oxidation and has good air stability and thermal stability; third, the raw material of alloyed tellurium oxide is cheap and has low cost, and is suitable for large-scale production by vacuum thermal evaporation deposition; therefore, this embodiment uses alloyed tellurium oxide as the hole transport layer, which can achieve a high-performance, high-stability and low-cost perovskite solar cell module.
[0079] The hole transport layer, perovskite light absorption layer, electron transport layer and metal electrode layer of this embodiment are all prepared by vacuum thermal evaporation deposition method, which is suitable for the preparation of large-area perovskite solar cell modules with high repeatability; first, in the vacuum thermal evaporation deposition method, the film is prepared under vacuum conditions, has excellent film uniformity, avoids contamination by impurities and gases, and is conducive to high performance and high stability of the film and the device; second, the preparation process can accurately control the film thickness, has high controllability and repeatability, does not contain toxic solvents, and has excellent device reproducibility and scalability, which is suitable for the preparation of large-area module devices, and significantly improves the high yield rate of industrial applications of perovskite solar cell modules; third, compared with other deposition technologies, the structure of the vacuum thermal evaporation equipment is relatively simple and the maintenance cost is low; therefore, the present invention realizes the preparation of perovskite solar cell modules by full vacuum thermal evaporation deposition method, which is conducive to the industrial development of perovskite solar cell modules.
[0080] Embodiment 2
[0081] On the basis of Example 1, this example provides an industrially applicable perovskite solar cell module, which is prepared by the preparation method of Example 1.
[0082] See also Figure 2h and Figure 3 , Figure 3 A top view of an industrial perovskite solar cell module provided in an embodiment of the present invention. The industrial perovskite solar cell module comprises: a substrate, a transparent electrode layer, a hole transport layer 2, a perovskite light absorption layer 3, an electron transport layer 4 and a metal electrode layer 5.
[0083] Among them, the transparent electrode layer is located on the substrate, and a plurality of first grooves p1 are formed in the transparent electrode layer, and the plurality of first grooves p1 divide the transparent electrode layer 1 into a plurality of sub-cell regions; the hole transport layer 2 is located on the surface of the middle sub-cell region 113 of the plurality of sub-cell regions, on a portion of the surface of the first end sub-cell region 111, and on a portion of the surface of the second end sub-cell region 112, and is filled in the plurality of first grooves p1; the material of the hole transport layer 2 includes alloyed tellurium oxide, and the alloyed tellurium oxide is formed by mixing any one of the alloy elements of Se, S, P, As, Mg, Fe, and Al with tellurium oxide; the perovskite light absorption layer 3 and the electron transport layer 4 are sequentially stacked on the surface of the hole transport layer 2; each middle sub-cell A second groove p2 is formed above the region 113, and the second groove p2 penetrates the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2; the metal electrode layer 5 fills a number of second grooves p2, and at the same time extends from the surface of the electron transport layer 4 to the surface of the second end sub-battery region 112; the metal electrode layer located on the surface of the first end sub-battery region 111 is a preset distance away from the hole transport layer to form an independent metal electrode 6; a third groove p3 is formed above each intermediate sub-battery region 113, and the third groove p3 penetrates the metal electrode layer 5, the electron transport layer 4, the perovskite light absorption layer 3 and the hole transport layer 2 to form a number of sub-batteries interconnected by the metal electrode layer 5 in the second groove p2.
[0084] In this embodiment, the material of the hole transport layer adopts alloyed tellurium oxide formed by mixing any one of the alloy elements of Se, S, P, As, Mg, Fe, and Al with tellurium oxide; first, the alloyed tellurium oxide has a high mobility, which can effectively improve the charge transfer capability of the perovskite solar cell module, thereby improving the efficiency of the large-area perovskite solar cell module; second, the alloyed tellurium oxide is an oxide material, which is insensitive to air oxidation and has good air stability and thermal stability; third, the raw material price of alloyed tellurium oxide is low and the cost is low, which is suitable for large-scale production by vacuum thermal deposition method; therefore, this embodiment adopts alloyed tellurium oxide as the hole transport layer, which can realize a high-performance, high-stability and low-cost perovskite solar cell module.
[0085] Embodiment 3
[0086] Based on Example 1 and Example 2, this example further illustrates a method for preparing a perovskite solar cell module for industrial application. The method for preparing a perovskite solar cell module for industrial application comprises the following steps:
[0087] S1, etching the transparent electrode layer 1 to form a plurality of first grooves p1, wherein the plurality of first grooves p1 divide the transparent electrode layer 1 into a plurality of sub-cell regions, such as Figure 2a and Figure 2b shown.
[0088] Specifically, first clean an area of 10×10cm 2 The ITO transparent electrode layer 1 is then laser etched, and the etching depth exceeds the thickness of the transparent electrode layer 1, so as to divide a number of sub-battery areas, the laser frequency is 400kHz, the etching speed is 2000mm / s, the etching times are 2 times, and the laser wavelength is 1064nm; finally, the transparent electrode layer 1 is placed in Decon-90 cleaning agent, deionized water, acetone, alcohol and deionized water in turn for ultrasonic cleaning, and after cleaning, it is blown dry with a nitrogen gun and placed in ultraviolet ozone for pretreatment. The cleaning temperature of ultrasonic cleaning is 50°C, and the time of each ultrasonic cleaning is 30min.
[0089] Further, two end regions among the plurality of sub-cell regions are respectively defined as a first end sub-cell region 111 and a second end sub-cell region 112 , and each region between the two ends is defined as an intermediate sub-cell region 113 .
[0090] S2, depositing hole transport materials on the surfaces of several sub-cell regions and in several first grooves p1 to form a hole transport layer 2, such as Figure 2c shown.
[0091] Specifically, the hole transport layer 2 was prepared by vacuum thermal evaporation deposition. The sample was fixed on a mask plate, 300 mg of TeO2 powder and 8 mg of Se powder were placed in the same crucible, the distance between the substrate baffle and the crucible was adjusted to 20 cm, and the vacuum was evacuated to 5×10 -4 Pa; set the corresponding parameters, among which the evaporation rate is set to 0.5Å / s, monitor the thickness of the Se alloyed Se-TeO2 hole transport layer 2 during the deposition process, and turn off the corresponding operations in sequence when it reaches 80nm, and take out the sample after the vacuum degree reaches atmospheric pressure; anneal the evaporated sample in an air environment at 225℃ for 30min.
[0092] In another embodiment, the type and quality of the alloying elements can be adjusted as required, for example, 300 mg TeO2 powder and 12 mg Se powder are placed in the same crucible, or 300 mg TeO2 powder and 16 mg Se powder are placed in the same crucible, or 300 mg TeO2 powder and 20 mg Se powder are placed in the same crucible, or 300 mg TeO2 powder and 24 mg Se powder are placed in the same crucible, or 300 mg TeO2 powder and 16 mg S powder are placed in the same crucible, or 300 mg TeO2 powder and 16 mg As powder are placed in the same crucible, or 300 mg TeO2 powder and 16 mg Mg powder are placed in the same crucible, or 300 mg TeO2 powder and 16 mg Fe powder are placed in the same crucible, or 300 mg TeO2 powder and 16 mg Al powder are placed in the same crucible.
[0093] In other embodiments, the annealing temperature of the evaporated sample can be adjusted as required, for example, the evaporated sample is annealed in an air environment at 200° C. for 30 min, or the evaporated sample is annealed in an air environment at 250° C. for 30 min.
[0094] S3, depositing a perovskite light absorbing layer 3 on the surface of the hole transport layer 2, such as Figure 2d shown.
[0095] The perovskite light-absorbing layer was prepared by sequential vacuum thermal evaporation deposition. The sample was fixed on a mask plate. First, 691.5 mg of PbI2 and 19.5 mg of CsI powder were placed in the same crucible. The distance between the substrate baffle and the crucible was adjusted to 20 cm. The vacuum was evacuated to 5×10 -4 Pa, wherein the evaporation rate was set to 1.0Å / s, and the corresponding operations were shut down one by one when the total thickness of (PbI2+CsI) was monitored to be 330nm during the deposition process; then 180mg of FAI powder was placed in the crucible, and the rest was the same as above, the evaporation rate was set to 1.0Å / s, and the corresponding operations were shut down one by one when the FAI thickness was monitored to be 230nm during the deposition process; finally, 28mg of MABr powder was placed in the crucible, and the rest was the same as above, the evaporation rate was set to 0.5Å / s, and the corresponding operations were shut down one by one when the MABr thickness was monitored to be 40nm during the deposition process; the sample was taken out after the vacuum degree reached atmospheric pressure, and the evaporated sample was annealed in an air environment at 120℃ for 20min.
[0096] The corresponding operation refers to the fixed operation of the instrument after the evaporation is completed, such as closing the substrate baffle, turning on the automatic shutdown, turning off the substrate rotation, closing the metal baffle, closing the ionization gauge when the speed reaches zero, opening the bleed valve, taking out the sample, closing the bleed valve, closing the hatch and turning on the mechanical pump, opening the bypass valve, and when the air pressure is below 10 Pa, closing the bypass valve, turning off the mechanical pump, and finally turning off the instrument.
[0097] S4, depositing an electron transport layer 4 on the surface of the perovskite light absorbing layer, such as Figure 2e shown.
[0098] The electron transport layer 4 was prepared by vacuum thermal evaporation deposition. The sample was fixed on a mask plate and 60 mg C was placed in a crucible. 60 Powder, adjust the distance between substrate baffle and crucible to 20cm, and evacuate to 5×10 -4 Pa; set the corresponding parameters, including setting the evaporation rate to 0.5Å / s, and monitoring C during the deposition process 60 When the thickness of the electron transport layer reaches 30nm, the corresponding operations are turned off in sequence. 20mg of BCP powder is placed in the crucible. Other operations are the same as above. When the BCP thickness is monitored to be 6nm during the deposition process, the corresponding operations are turned off in sequence. The sample is taken out after the vacuum degree reaches atmospheric pressure.
[0099] S5, etching to form a second trench p2, such as Figure 2f shown.
[0100] The second groove p2 is etched by laser scribing. The etching depth is the vertical distance from the film surface to the ITO transparent electrode layer 1, so that the bottom ITO transparent electrode layer 1 is exposed, and the interconnection position is reserved. The laser frequency is 1000kHz, the etching speed is 800mm / s, the etching number is 1, and the laser wavelength is 355nm.
[0101] S6, depositing a metal electrode layer 5, such as Figure 2g shown.
[0102] The Cu electrode was prepared by vacuum thermal evaporation deposition method and the vacuum was 5×10 -4 Pa; set the corresponding parameters, among which the evaporation rate was set to 0.8Å / s, and monitor the thickness of the Cu electron transport layer during the deposition process. When the thickness reaches 150nm, shut down the corresponding operations in sequence, and take out the sample after the vacuum degree reaches atmospheric pressure.
[0103] S7, etching to form independent metal electrodes 6 and third trenches p3, and obtaining a plurality of sub-cells interconnected by the metal electrode layer 5 in the second trenches p2, such as Figure 2h shown.
[0104] The third groove p3 is formed by etching with a laser scribing method, and the etching depth is the total thickness from the metal electrode layer 5 to the hole transport layer 2, thereby cutting off the metal electrode layer 5 and separating the sub-cells, so that the sub-cells are interconnected only through the metal electrode layer 5 in the second groove p2, wherein the laser frequency is 600kHz, the etching speed is 2400mm / s, the etching times is 1, and the laser wavelength is 355nm. At this point, the preparation of a large-area perovskite solar cell module is completed.
[0105] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a perovskite solar cell module for industrial application, characterized in that: Includes steps: S1, etching the transparent electrode layer to form a plurality of first grooves, wherein the plurality of first grooves divide the transparent electrode layer into a plurality of sub-cell regions; S2. Using a vacuum thermal evaporation deposition method, tellurium oxide powder and alloy element powder are used as raw materials to deposit hole transport materials on the surfaces of the plurality of sub-cell regions and in the plurality of first grooves to form a hole transport layer, and annealing the hole transport layer in air at a temperature of 150-250° C.; wherein the material of the hole transport layer includes alloyed tellurium oxide, the alloyed tellurium oxide is formed by mixing tellurium oxide with any one of Se, S, P, As, Mg, Fe, and Al alloy elements, the mass of the tellurium oxide is 280-320 mg, and the mass of the alloy element is 8-24 mg; S3, depositing a perovskite light absorbing layer on the surface of the hole transport layer by a vacuum thermal evaporation deposition method; S4, depositing an electron transport layer on the surface of the perovskite light absorbing layer by a vacuum thermal evaporation deposition method; S5, etching the electron transport layer, the perovskite light absorption layer and the hole transport layer until the transparent electrode layer, exposing a portion of the surface of the first end sub-cell region and a portion of the surface of the second end sub-cell region in the plurality of sub-cell regions, and forming a second groove above the middle sub-cell region of the plurality of sub-cell regions; S6. Depositing a metal electrode layer by vacuum thermal evaporation deposition, wherein one end of the metal electrode layer extends from the surface of the electron transport layer to the surface of the first end sub-battery region, and the other end of the metal electrode layer extends from the surface of the electron transport layer to the surface of the second end sub-battery region, and is filled in the second groove; S7. Etch the metal electrode layer of the first end sub-cell region until the transparent electrode layer, so that the metal electrode layer on the surface of the first end sub-cell region is at a preset distance from the hole transport layer, and at the same time, etch the metal electrode layer, electron transport layer, perovskite light absorption layer and hole transport layer above each intermediate sub-cell region until the transparent electrode layer to form a third groove, to obtain a plurality of sub-cells interconnected by the metal electrode layer in the second groove.
2. The method for preparing an industrially applicable perovskite solar cell module according to claim 1, characterized in that: Step S1 includes: Laser etching the transparent electrode layer, with an etching depth greater than or equal to the thickness of the transparent electrode layer, to form the plurality of first grooves; wherein the laser frequency is 300-500 kHz, the etching speed is 1800-2200 mm / s, the etching times is 2 times, and the laser wavelength is 1064 nm; The transparent electrode layer is cleaned.
3. The method for preparing an industrially applicable perovskite solar cell module according to claim 1, characterized in that: Step S2 includes: Using vacuum thermal evaporation deposition method, the vacuum pressure is 3×10 -4 -5×10 -4 Pa, the evaporation rate is Under the conditions of , depositing 70-90 nm of hole transport material on the surfaces of the plurality of sub-cell regions and in the plurality of first grooves to form a hole transport layer; The hole transport layer is annealed in air at a temperature of 150-250° C. for 20-40 minutes.
4. The method for preparing an industrially applicable perovskite solar cell module according to claim 1, characterized in that: The general structural formula of the perovskite light absorbing layer material is ABX3, wherein A is a cation and A is selected from MA + , FA + , Rb + , Cs + One or more of; B is a cation and B is selected from Pb 2+ Sn 2+ One or more of; C is an anion and is selected from Cl - Br - ,I - One or more of; When the perovskite light absorbing layer is Cs 0.05 FA 0.70 MA 0.25 PbI 2.75 Br 0.25 When , step S3 includes: Using vacuum thermal evaporation deposition method, at a pressure of 3×10 -4 -5×10 -4 Pa, the evaporation rate is Under the conditions of, depositing PbI2 and CsI with a total thickness of 310-350nm on the surface of the hole transport layer; then at an evaporation rate of 210-250nm FAI was deposited under the conditions of ; finally, at an evaporation rate of 30-50 nm MABr was deposited under the conditions of ; and annealed in air environment at 110-130 ° C for 15-30 min to obtain a composition of Cs 0.05 FA 0.70 MA 0.25 PbI 2.75 Br 0.25 Perovskite light-absorbing layer.
5. The method for preparing an industrially applicable perovskite solar cell module according to claim 1, characterized in that: Step S4 includes: Using vacuum thermal evaporation deposition method, at a pressure of 3×10 -4 -5×10 -4 Pa, the evaporation rate is Under the conditions of , 20-40nm of electron transport material is deposited on the surface of the perovskite light absorbing layer, and then at a evaporation rate of Under the conditions of , 5-10 nm of interface modification material is deposited to form the electron transport layer.
6. The method for preparing an industrially applicable perovskite solar cell module according to claim 1, characterized in that: Step S5 includes: Laser etching the electron transport layer, the perovskite light absorption layer and the hole transport layer until the transparent electrode layer, exposing a portion of the surface of the first end sub-cell region and a portion of the surface of the second end sub-cell region in the plurality of sub-cell regions, and forming a second groove above the middle sub-cell region of the plurality of sub-cell regions; Among them, the laser frequency is 800-1200kHz, the etching speed is 600-1000mm / s, the etching number is 1 time, and the laser wavelength is 355nm.
7. The method for preparing an industrially applicable perovskite solar cell module according to claim 1, characterized in that: Step S6 includes: Using vacuum thermal evaporation deposition method, at a pressure of 3×10 -4 -5×10 -4 Pa, the evaporation rate is A 130-160nm metal electrode layer is deposited under the conditions.
8. The method for preparing an industrially applicable perovskite solar cell module according to claim 1, characterized in that: Step S7 includes: Laser etching the metal electrode layer of the first end sub-cell region to the transparent electrode layer, so that the metal electrode layer on the surface of the first end sub-cell region is at a preset distance from the hole transport layer, and laser etching the metal electrode layer, the electron transport layer, the perovskite light absorption layer and the hole transport layer above each intermediate sub-cell region to the transparent electrode layer to form a third groove, thereby obtaining a plurality of sub-cells interconnected by the metal electrode layer in the second groove; Among them, the laser frequency is 400-800kHz, the etching speed is 2200-2600mm / s, the etching number is 1 time, and the laser wavelength is 355nm.
9. An industrial application of perovskite solar cell module, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8, comprising: a substrate, a transparent electrode layer, a hole transport layer, a perovskite light absorption layer, an electron transport layer and a metal electrode layer, wherein: The transparent electrode layer is located on the substrate, and a plurality of first grooves are formed in the transparent electrode layer, and the plurality of first grooves divide the transparent electrode layer into a plurality of sub-cell regions; The hole transport layer is located on the surface of the middle sub-cell region among the plurality of sub-cell regions, a portion of the surface of the first end sub-cell region, and a portion of the surface of the second end sub-cell region, and is filled in the plurality of first grooves; the material of the hole transport layer includes alloyed tellurium oxide, the alloyed tellurium oxide is formed by mixing tellurium oxide with any one of the alloy elements of Se, S, P, As, Mg, Fe, and Al, the mass of the tellurium oxide is 280-320 mg, and the mass of the alloy element is 8-24 mg; The perovskite light absorption layer and the electron transport layer are sequentially stacked on the surface of the hole transport layer; a second groove is formed above each of the intermediate sub-cell regions, and the second groove runs through the electron transport layer, the perovskite light absorption layer and the hole transport layer; The metal electrode layer fills a plurality of the second grooves and extends from the surface of the electron transport layer to the surface of the second end sub-battery region; the metal electrode layer located on the surface of the first end sub-battery region is at a preset distance from the hole transport layer; A third groove is formed above each of the intermediate sub-cell regions, and the third groove penetrates the metal electrode layer, the electron transport layer, the perovskite light absorption layer and the hole transport layer to form a plurality of sub-cells interconnected by the metal electrode layer in the second groove.
Citation Information
Patent Citations
Perovskite battery assembly, preparation method and application thereof
CN112952009A
Photoelectric device, preparation method thereof and display terminal
CN115802786A
Heterogeneous crystalline silicon solar cell, preparation method and photovoltaic device
CN117594686A