A method for recycling waste solid composite propellant
By mixing waste solid composite propellant with fly ash and other substances to form a slurry fluid and incinerate at high temperature, the safety and environmental pollution problems of waste treatment are solved, and efficient recycling and resource utilization of aluminum elements are achieved to achieve environmental protection and Efficient treatment effect.
Patent Information
- Application Number
- CN202411143196.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The prior art cannot effectively and safely deal with waste solid composite propellants, resulting in environmental pollution and waste of resources. Traditional methods have safety hazards and air pollution problems.
The waste solid composite propellant is mixed with fly ash, water and additives in a certain proportion, and then the slurry fluid is formed and the flue gas is incinerated through a high-temperature dust collector and deacidification tower. The aluminum is recovered by hydrochloric acid leaching method to achieve ash Harmless treatment of slag.
It has achieved safe and environmentally friendly treatment of waste, improved storage and transportation stability, reduced environmental pollution, promoted the resource reuse of aluminum elements, and achieved national emission standards, and the aluminum recovery rate was as high as more than 93%.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid composite propellant recovery, and in particular relates to a method for recovering waste solid composite propellant. Background Art
[0002] Composite propellant is a high-energy-density fuel widely used in rockets, missiles and other weapons and equipment. However, during the production and storage process, due to the influence of time and storage conditions, solid composite propellants may experience surface hardening, interface shedding, density reduction, loss of energetic components, etc. Therefore, generally after 5 to 10 years, the aged composite solid composite propellant will enter the scrap period.
[0003] At present, the traditional methods for treating waste solid composite propellants mainly include deep soil burial, dumping in the high seas, open-air burning and explosion. However, these methods have great safety and environmental problems. Landfill and dumping will cause a certain degree of damage to the entire ecosystem, and there are still certain safety hazards. Open-air burning and explosion methods will cause the generation of harmful substances such as particulate matter, nitrogen oxides, and chlorine-containing gases during the combustion process, which will have different degrees of impact on the atmospheric environment. Therefore, it is of great practical significance to recover and recycle the effective components of composite propellants.
[0004] Patent CN110283354A discloses a degradation solvent and application for scrapped hydroxy-terminated polybutadiene composite solid propellant, which uses xylene and ketone solvents to initially swell the solid propellant, and then adds inorganic bases for degradation. However, the degradation process takes a long time, and the degraded material needs to be separated into oil and water, and the water phase and oil phase need to be treated separately, which is a relatively complicated process.
[0005] Patent CN106414316A discloses a method for treating spent solid rocket propellant, wherein spent rocket propellant containing ammonium perchlorate, powdered aluminum, a rubber-based adhesive and a small amount of remaining mixture is treated by disintegration, leaching and crystallization to recover ammonium perchlorate. However, this method does not recover other components in the solid propellant, and the recovery is relatively limited. In addition, the separated inert materials and solid residues are not properly handled in subsequent processing, which may cause secondary pollution.
[0006] Therefore, finding a new waste solid composite propellant disposal technology that can make waste solid composite propellants safe, harmless, reduced in volume, and resource-based is a technical problem that needs to be solved. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a method for recovering waste solid composite propellant.
[0008] The technical means adopted by the present invention are as follows:
[0009] A method for recovering waste solid composite propellant comprises the following steps:
[0010] S1. The composite propellant, fly ash, water and additives are mixed and stirred uniformly in a mass ratio of (25.5 ~38.6): (28~54.5): (20~33.3): (0.3~0.5) to obtain a slurry fluid;
[0011] S2. The slurry fluid is sent to the combustion furnace for combustion. The gas generated by the combustion passes through a high-temperature dust collector to separate the inorganic ash in the flue gas, and then enters a deacidification tower to remove the acid gas in the flue gas; the purified flue gas is discharged through the top of the tower to meet the standards. The inorganic ash generated by the combustion is used to recover aluminum through a hydrochloric acid leaching method.
[0012] Preferably, the composite propellant is a hydroxyl-terminated composite propellant, and the composite propellant is ground to a particle size of less than 1 mm before mixing.
[0013] Preferably, the aluminum-containing powder is a powder material having an average particle size of less than 75 μm and an aluminum content of more than 5 wt%, such as aluminum oxide powder, coal gasification fine slag, slag powder, etc.
[0014] Preferably, the aluminum-containing powder is fly ash, and the mass proportion of the fly ash with a particle size below 30 μm accounts for more than 85% of the total fly ash content.
[0015] Preferably, the dispersant is sodium humate and / or sodium lignin sulfonate.
[0016] Preferably, in step S1, the stirring speed is 500 r / min-700 r / min, and the stirring is performed for 10 min-15 min.
[0017] Preferably, in step S2, the incineration temperature is >850°C; the pressure of the furnace pressurized incineration is <0.5MPa; and the furnace combustion residence time is ≥8s.
[0018] Preferably, the method for treating the gas generated by combustion is that the gas generated by combustion passes through a high-temperature dust collector to separate inorganic ash in the flue gas, and then enters a deacidification tower to remove acidic gases in the flue gas; the purified flue gas is discharged through the top of the tower to meet the standards.
[0019] Preferably, the inorganic ash produced by the combustion is treated by mixing fly ash with HCl solution, separating silicon and aluminum by sedimentation separation, removing iron and calcium ions from the filtrate by a resin impurity removal system, concentrating and crystallizing, and obtaining Al2O3 product by roasting.
[0020] The beneficial effects of the present invention are as follows:
[0021] 1) This recycling method adds appropriate amounts of aluminum-containing powder, water and additives to scrapped solid composite propellants, mixes and stirs the waste in a certain proportion to form a slurry fluid, which can prevent the occurrence of dangerous situations such as natural ignition and dust flying of solid waste, improve its storage, pumping and atomization stability, achieve complete control of the combustion recovery process and tail gas treatment, realize harmless treatment of combustion ash, and solve the problems of difficult recycling and treatment of waste solid composite propellants and serious environmental pollution.
[0022] 2) Fly ash is preferred as the aluminum-containing powder. On the one hand, the doped fly ash can support the large-sized propellant particles, so that the slurry has good fluidity while maintaining good stability; on the other hand, after combustion, the main component of the solid residue after the propellant is Al2O3, which can be mixed with fly ash to increase the aluminum content in the fly ash. Subsequently, it can be properly disposed of or recycled in accordance with relevant regulations to achieve harmless treatment of combustion ash.
[0023] 3) The gas components such as H2O, CO2, NOx, SOx, etc. generated during the combustion process can be easily processed to meet the emission standards through existing mature technologies and discharged into the atmosphere.
[0024] 4) This method provides an efficient and environmentally friendly solution for the treatment of solid composite propellant waste, which is of great significance for improving waste treatment efficiency, reducing environmental pollution and promoting resource recycling. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is described in more detail below in conjunction with the embodiments.
[0026] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this article can be purchased from the market or prepared by existing methods.
[0027] First, a slurry fluid was prepared by weighing a certain amount of fly ash and waste solid composite propellant, feeding them into a mixing tank through a screw conveyor, adding water and slurrying auxiliary materials in a certain proportion, turning on the agitator in the mixing tank, and stirring evenly for 10 min at a speed of 500 r / min to obtain a slurry fluid.
[0028] According to the above operation, 9 groups of slurry fluids in Examples 1-9 were prepared respectively.
[0029] The composite propellant formula used in Examples 1, 2 and 3 is: 35.71wt% of terminal hydroxyl polybutadiene, 23.21wt% of ammonium perchlorate, 5.36wt% of cyclotrimethylene trinitramine, 3.57wt% of toluene diisocyanate, 10.71wt% of dioctyl sebacate, and 21.43wt% of aluminum.
[0030] The composite propellant formula used in Examples 4, 5 and 6 is: 37.74 wt % of terminal hydroxyl polybutadiene, 24.53 wt % of ammonium perchlorate, 3.77 wt % of toluene diisocyanate, 11.32 wt % of dioctyl sebacate, and 22.64 wt % of aluminum.
[0031] The composite propellant formula used in Examples 7, 8 and 9 is: 46.51 wt% of terminal hydroxyl polybutadiene, 6.98 wt% of cyclotrimethylene trinitramine, 4.65 wt% of toluene diisocyanate, 13.95 wt% of dioctyl sebacate, and 27.91 wt% of aluminum.
[0032] The composition and proportion of the composite propellant, fly ash (the mass proportion of particles with a diameter of less than 30 μm accounts for more than 85% of the total fly ash content), water and additives are shown in Table 1 below.
[0033] Table 1 Solid composite propellant slurry formulation (wt%)
[0034] ;
[0035] The slurries prepared in Examples 1-9 were subjected to viscosity tests, stability tests and calorific value tests. The apparent viscosity of the slurries was measured using a NXS-4C water-coal slurry viscometer (Chengdu Instrument Factory), the temperature was set at 25 °C, and the volume of each measurement was about 25 ml of slurry, and the shear rate was 100 s -1 The apparent viscosity under the condition of 1.5 ℃ is 2.5 ℃. Take an appropriate amount of the prepared slurry and put it into a test tube. The slurry in the test tube is about 20 ml and sealed with a lid. The time is considered to be 7 days, and the water precipitation rate of the slurry is observed. The high calorific value of the slurry is determined by oxygen bomb calorimetry. The test results are shown in Table 2 below.
[0036] Table 2 Performance test of slurry prepared in Examples 1-9
[0037] ;
[0038] It can be seen that the viscosity of the slurry prepared in all embodiments is lower than 600 mPa.s, which is conducive to pipeline transportation and atomization, and achieves the purpose of good combustion; at the same time, the water separation rate of the slurry is below 11.5%, which will be more stable during storage and transportation, and can reduce the stratification and precipitation problems that may be caused by water separation; the calorific value of the prepared slurry is between 19.51 and 25.01 MJ / kg, which is close to the calorific value of standard coal 29.27 MJ / kg.
[0039] Furthermore, the slurried fluid is fed into a combustion furnace for combustion.
[0040] The slurries prepared in Examples 1, 4, and 7 were respectively fed to the feed inlet of the pressurized fluidized bed incinerator at a feed rate of 15 kg / h, and sprayed into the furnace through 200 kPa compressed air. The incineration temperature was >850°C, the pressure of the pressurized incineration in the furnace was <0.5 MPa, and the residence time of the furnace combustion was ≥8s. The generated high-temperature flue gas and the burned inorganic ash were discharged through the flue at the top of the incinerator. The high-temperature wet flue gas generated by the combustion passed through the high-temperature dust collector to separate the inorganic ash in the flue gas, and the discharged flue gas continued to enter the deacidification tower to remove the acidic gas in the flue gas; the generated purified flue gas was discharged through the top of the tower to meet the standards.
[0041] The nitrogen oxide concentrations in the flue gas at various locations detected by the flue gas analyzer are shown in Table 3.
[0042] Table 3 Nitrogen oxide concentrations in flue gas at various locations
[0043] ;
[0044] It can be seen that after the flue gas in the three embodiments passes through the high-temperature dust collector to separate the inorganic ash in the flue gas and the deacidification tower to remove the acid gas in the flue gas, the nitrogen oxide content drops to below 42 ppm, which is lower than the national nitrogen oxide emission standard of 50 ppm.
[0045] Fly ash, water and additives were mixed and stirred evenly in a mass ratio of 71.2:28.4:0.4 to obtain a slurry fluid, which was recorded as Comparative Example 1.
[0046] XRF test was performed on the fly ash and inorganic ash after combustion in the slurry prepared in Examples 1, 4, 7 and Comparative Example 1. The content of aluminum in the fly ash before combustion and the inorganic ash after combustion is shown in Table 4 below.
[0047] Table 4 Elemental analysis of slurries prepared in Examples 1, 4, 7 and Comparative Example 1 before and after combustion
[0048] ;
[0049] The aluminum content in the inorganic ashes of Examples 1, 4 and 7 is significantly higher than that in the fly ash, and the aluminum content exceeds 25.985%. However, the aluminum content in Comparative Example 1 is only 16.012%, indicating that the increase in the aluminum content in the inorganic ashes is mainly caused by the solid residue after the propellant is burned.
[0050] Hydrochloric acid with a concentration of 4.95 mol / L and inorganic ash were placed in a reactor at a liquid-solid ratio of 5:1 for reaction. The temperature was controlled at 95°C and the reaction time was 3 h. After the reaction, the filtrate was filtered, and the filtrate was heated, concentrated and crystallized after removing iron and calcium ions through a resin impurity removal system. The crystallized aluminum chloride was roasted at 1200°C for 4 h to obtain Al2O3. The filtered residue and Al2O3 were tested by XRF, and the aluminum leaching rate from the ash and the purity of Al2O3 were calculated, as shown in Table 5.
[0051] Table 5 Aluminum leaching rate and Al2O3 purity in ash
[0052] ;
[0053] It can be seen that the Al content of the ash in the three examples is 3+ The leaching rates all exceeded 93%, indicating that the utilization efficiency of the raw materials in the leaching process was high, reducing the waste of resources. At the same time, the purity of Al2O3 was quite high in the three embodiments, all exceeding 96%.
[0054] The above experiments show that the viscosity, stability and calorific value of the slurry made from composite propellant waste meet the GB 50360-2016 standard. It can also prevent the occurrence of dangerous situations such as natural ignition of solid waste and flying dust. The aluminum content in the ash after combustion is significantly higher than that in the fly ash before combustion, which is conducive to the enrichment and recovery of aluminum. The dust particles in the flue gas purified by the high-temperature dust collector can be reduced to 5 mg / m 3 After passing through the deacidification tower, the nitrogen oxide content is 40 ppm, which is lower than the national nitrogen oxide emission standard of 50 ppm; the aluminum in the fly ash is recovered by hydrochloric acid leaching method, and the leaching rate of aluminum in the ash can reach more than 93.52%, and the Al2O3 purity is above 95.8%.
[0055] The above implementation modes are only used to illustrate the technical solutions of the present invention, but not to limit the present invention. Although the present invention has been described in detail with reference to the above implementation modes, those skilled in the art should understand that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for recovering waste solid composite propellant, characterized in that: The following steps are involved: S1. The composite propellant, aluminum-containing powder, water, and additive are mixed and stirred uniformly in a mass ratio of (25.5-38.6): (28-54.5): (20-33.3): (0.3-0.5) to obtain a slurry fluid; S2. The slurry fluid is sent to a combustion furnace for combustion. After the inorganic ash is separated, the flue gas generated by the combustion enters a deacidification tower to remove the acidic gas in the flue gas and then is discharged. The inorganic ash generated by the combustion is used to recover aluminum by hydrochloric acid leaching; The aluminum-containing powder is aluminum oxide powder or coal gasification fine slag or slag powder.
2. The method for recycling waste solid composite propellant according to claim 1, characterized in that: The composite propellant is a hydroxyl-terminated composite propellant, and the composite propellant is ground to a particle size of less than 1 mm before mixing.
3. The method for recycling waste solid composite propellant according to claim 1, characterized in that: The aluminum-containing powder is a powder material with an average particle size of less than 75 μm and an aluminum content of more than 5 wt %.
4. A method for recycling waste solid composite propellant according to claim 3, characterized in that: The aluminum-containing powder is fly ash, and the mass proportion of the fly ash with a particle size below 30 μm accounts for more than 85% of the mass of the entire fly ash.
5. The method for recycling waste solid composite propellant according to claim 1, characterized in that: The additive is sodium humate and / or sodium lignin sulfonate.
6. The method for recycling waste solid composite propellant according to claim 1, characterized in that: In step S1, the stirring speed is 500 to 700 r / min, and the stirring time is 10 to 15 min.
7. The method for recycling waste solid composite propellant according to claim 1, characterized in that: In the step S2, the pressure of the pressurized incineration in the furnace of the combustion furnace is less than 0.5 MPa, the combustion temperature in the furnace is higher than 850°C, and the combustion residence time of the slurry fluid in the furnace is at least 8 s.
8. The method for recycling waste solid composite propellant according to claim 1, characterized in that: The flue gas is separated into inorganic ash in a high-temperature dust collector.
9. The method for recycling waste solid composite propellant according to claim 1, characterized in that: The hydrochloric acid leaching method for recovering aluminum is as follows: inorganic ash is subjected to magnetic separation to remove iron, then mixed with HCl solution for reaction, allowed to settle, filtered to obtain filtrate; the filtrate is subjected to resin to remove impurities, concentrated and crystallized, and the crystals are roasted to obtain Al2O3 products.