A high specific capacity sodium ion manganese-based positive electrode material, its precursor and preparation method
The synthesis of sodium ion layered manganese-based oxide positive electrode material through four-step method has solved the problem of low actual discharge specific capacity and poor circulation performance in sodium ion batteries, achieved high specific capacity and good rate performance, and improved sodium ion manganese Applicability of base oxide positive electrode material.
Patent Information
- Application Number
- CN202411180524.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing sodium ion layered manganese-based oxide positive electrode materials have low actual discharge capacity and poor circulation performance in sodium ion secondary batteries, which affect their application.
The sodium ion layered manganese-based oxide positive electrode material was synthesized by the four-step method. First, the manganese-based hydroxide with uniform distribution of transition metal Mn and other metal element M was synthesized by co-precipitation method, and then the sodium-containing hydroxide was synthesized by high-temperature solid-phase oxidation method. The ionic manganese-based precursor is then embedded in sodium by solvent thermal reduction method, and finally the high-temperature solid phase synthesizes a manganese-based positive electrode material for high-capacity sodium ion batteries.
Improves the first discharge capacity and cycling performance of sodium ion manganese-based cathode material, and can charge and discharge in the voltage range of 1.75~4.4V in room temperature, the first discharge capacity reaches more than 150mAh/g at 0.1C, and the discharge capacity still reaches 120mAh at 2.0C. /g, the capacity retention rate of 100 weeks of circulation reaches more than 95%.
Smart Images

Figure CN118684283B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials for sodium ion secondary batteries, and in particular to a high-specific-capacity sodium ion manganese-based positive electrode material, a precursor thereof, and a preparation method thereof. Background Art
[0002] Sodium ion batteries (SIBs) have attracted extensive attention from the scientific and industrial communities due to their abundant raw material resources and low cost. Cathode materials are key components that affect the voltage, capacity, and cycle life of SIBs. x Mn y M 1-y O2 (0< x ≤1, y >0.5, M is Ni, Co, Mg, Cu, Fe, etc.) can be divided into tunnel-type and layered transition metal oxides according to the sodium content and crystal structure. Although the former has good stability, it has a low specific capacity. Layered manganese-based oxide positive electrode materials have become one of the most promising sodium ion positive electrode materials for commercialization due to their low cost, simple synthesis method and high theoretical specific capacity.
[0003] Although sodium ion layered manganese-based oxide positive electrode materials have the advantages of low raw material cost and high theoretical specific capacity, there are still some problems that affect their practical application, such as low actual specific capacity, poor structural stability, insufficient cycle performance and rate performance.
[0004] By improving the synthesis process of sodium-ion layered manganese-based oxide cathode materials, their electrochemical performance can be improved. The traditional method for preparing sodium-ion layered manganese-based oxide cathode materials is to use a one-step high-temperature solid-phase method. Although this method is simple, the actual discharge capacity of the synthesized sodium-ion layered manganese-based oxide cathode materials is low, and the cycle performance and rate performance are poor.
[0005] Therefore, it is crucial to invent a new synthesis process for sodium ion layered manganese-based oxide positive electrode materials, improve the current problems of low actual discharge specific capacity, poor cycle performance and rate performance of sodium ion layered manganese-based oxide positive electrode materials, and improve the applicability of sodium ion layered manganese-based oxide positive electrode materials in the field of sodium ion secondary batteries. Summary of the Invention
[0006] The present invention provides a high-specific-capacity sodium-ion manganese-based positive electrode material, a precursor thereof, and a preparation method thereof, in order to solve the technical problems of low actual discharge specific capacity, poor cycle performance, and rate performance of existing manganese-based positive electrode materials for sodium-ion batteries.
[0007] To achieve the above object, the present invention provides a sodium ion-containing manganese-based precursor, which is prepared by embedding sodium ions into manganese-based hydroxide. The general formula of the sodium ion-containing manganese-based precursor is Na x Mny M 1-y O z , 0 <x≤0.5、0.5≤ y ≤1, 1≤z≤3; wherein M is any one or more of Ni, Co, Ti, Fe, Zn, Al, Cu, Nb, Ta, V, Cr, Sn, Si, Mo, W, Te, Mg, B, Zr, and Y, and the valence of Mn is +4.
[0008] Preferably, the preparation method comprises the following steps:
[0009] S1, according to the general formula of manganese-based precursor containing sodium ions Na x Mn y M 1-y O z Weigh a soluble salt of manganese element, a soluble compound containing element M, or a soluble salt containing metal element M in a stoichiometric ratio of the elements in the mixture, and add the soluble salt of manganese element and the soluble salt of element M into water to prepare a mixed solution;
[0010] The mixed solution, the precipitant solution and the buffer solution are added into the reactor simultaneously by a constant flow pump, the reaction conditions are controlled to obtain a coprecipitate, and the precipitate is filtered, washed and dried to obtain manganese-based hydroxide.
[0011] S2, according to the general formula of manganese-based precursor containing sodium ions Na x Mn y M 1-y O z The sum of the amounts of Mn and M in x Weigh a sodium source compound, and then evenly mix the sodium source compound with the manganese-based hydroxide obtained in step S1 to obtain a mixture;
[0012] Under the condition of continuous introduction of oxidizing gas, the mixture is heated to 200-800°C at a heating rate of 0.5-10°C / min, kept at this temperature for 1-48 hours, and cooled to obtain a manganese-based precursor containing sodium ions Na x Mn y M 1-y O z .
[0013] Preferably, in step S1, the soluble salt of manganese element is one or a combination of manganese chloride, manganese sulfate, manganese nitrate or manganese acetate;
[0014] The buffer is one or a combination of ethylenediamine, ammonia water, hydroxylammonium hydrochloride, sodium sulfosalicylate, sodium phosphate, ethylenediaminetetraacetic acid, hydroxyethylethylenediaminetriacetic acid, ethylene glycol bis(2-aminoethyl ether)tetraacetic acid, diethylenetriaminepentaacetic acid, and 1,2-cyclohexanediaminetetraacetic acid; and the precipitant is sodium hydroxide.
[0015] Preferably, in step S2, the sodium source compound is one or a combination of sodium carbonate, sodium oxide, sodium peroxide, sodium hydroxide, sodium nitrate, sodium bicarbonate or sodium oxalate;
[0016] Oxidizing gases are gases containing more than 10% oxygen or ozone.
[0017] A manganese-based sodium ion positive electrode material is prepared by using the above-mentioned manganese-based precursor containing sodium ions as a raw material and adopting a solvent thermal reduction method to synthesize a manganese-based sodium ion intermediate, and then calcining the manganese-based sodium ion intermediate at a high temperature;
[0018] The general formula of manganese-based sodium ion positive electrode material is Na n Mn y M 1-y O2, 0.5 <n≤1.5、0.5< y ≤1, wherein M is any one or more of Ni, Co, Ti, Fe, Zn, Al, Cu, Nb, Ta, V, Cr, Sn, Si, Mo, W, Te, Mg, B, Zr, and Y, and the valence of Mn is +3.
[0019] A method for preparing the above-mentioned manganese-based sodium ion positive electrode material comprises the following steps:
[0020] (1) According to the sodium ion-containing manganese-based positive electrode material Na n Mn y M 1-y O z Weigh the sodium source compound at 0.5 to 1.5 times the sum of the amount of Mn and M in the solution, and then mix the sodium source compound, the reducing agent and the sodium ion-containing manganese-based precursor Na x Mn y M 1-y O z Mix well to obtain a mixture;
[0021] (2) Under the protection of an inert gas atmosphere, the mixture is added into a reaction kettle containing water and an organic reagent as solvents, and the reaction is carried out at a temperature of 50-300°C for 1-48 hours. The manganese-based sodium ion intermediate is obtained by filtering, washing, and drying;
[0022] (3) Using the manganese-based sodium ion intermediate as the raw material, heat it to 200~500℃ at a heating rate of 0.5~10℃ / min under vacuum or inert atmosphere, and keep it warm for 2~30h; then heat it to 600~1200℃ at a heating rate of 0.5~10℃ / min, calcine it for 2~60h, and cool it down to obtain the manganese-based sodium ion positive electrode material Na n Mn y M 1-y O2.
[0023] Preferably, in step (1), the sodium source compound is one or a combination of sodium carbonate, sodium oxide, sodium peroxide, sodium hydroxide, sodium nitrate, sodium bicarbonate or sodium oxalate.
[0024] Preferably, in step (1), the reducing agent is one or a combination of ascorbic acid, glucose, sodium borohydride, sodium sulfite, sodium thiosulfate, magnesium, aluminum, zinc, tin, iron, oxalic acid, acetic acid, and aldehyde organic compounds.
[0025] Preferably, in steps (2) and (3), the inert gas is one or a combination of gases selected from nitrogen, argon, helium, hydrogen, and carbon dioxide with a purity of more than 99%.
[0026] The present invention provides a high specific capacity sodium ion manganese-based cathode material, a precursor thereof, and a preparation method thereof, which have the following beneficial effects:
[0027] (1) The innovation of the present invention adopts a four-step method to synthesize sodium ion layered manganese-based oxide positive electrode materials. During the synthesis process, a manganese-based hydroxide with a uniform distribution of transition metal Mn and other metal elements M is first synthesized by co-precipitation method, and then a sodium ion-containing manganese-based precursor is synthesized by high-temperature solid-phase oxidation method. Then, the sodium ion-containing manganese-based precursor is used as a raw material for solvent thermal reduction to insert sodium to synthesize a sodium ion manganese-based intermediate. Finally, a high-temperature solid-phase method is used to synthesize a high-capacity manganese-based positive electrode material for sodium ion batteries.
[0028] (2) Manganese-based positive electrode material Na for sodium ion battery prepared by the present invention n Mn y M 1-y O2, when charged and discharged in the voltage range of 1.75~4.4V at room temperature, the first discharge capacity is more than 150mAh / g at a rate of 0.1C (1.0C=100mA / g); the discharge capacity of this sodium ion manganese-based positive electrode material is still 120mAh / g at a rate of 2.0C, and the discharge capacity at a rate of 2.0C is still 80% of that at a rate of 0.1C; the capacity retention rate of this sodium ion manganese-based positive electrode material after 100 cycles at a rate of 0.5C is more than 95%. Therefore, this sodium ion manganese-based positive electrode material has good rate and cycle performance and can be used in sodium ion batteries.
[0029] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is the XRD pattern of the sodium ion manganese-based positive electrode material prepared in Example 1;
[0031] Figure 2 This is a first charge and discharge curve diagram of the sodium ion manganese-based positive electrode material prepared in Example 1;
[0032] Figure 3 This is a rate performance diagram of the sodium ion manganese-based positive electrode material prepared in Example 1;
[0033] Figure 4 This is a cycle performance diagram of the sodium ion manganese-based positive electrode material prepared in Example 1. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solutions and advantages disclosed in the embodiments of the present invention more clear, the embodiments of the present invention are further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the embodiments of the present invention and are not intended to limit the embodiments of the present invention. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0035] Example 1
[0036] A high specific capacity sodium ion manganese-based cathode material, its precursor and preparation method, comprising the following steps:
[0037] S1. Weigh 253.6 g of manganese sulfate monohydrate and 131.6 g of nickel sulfate hexahydrate, and add them to 1.0 L of water to prepare a mixed metal solution.
[0038] Add 160 g of sodium hydroxide and 10 mL of ethylenediamine solution (98%) to 1.0 L of water to obtain a sodium hydroxide mixed alkaline solution.
[0039] The mixed metal solution and the mixed alkali solution were added to the reactor simultaneously by a constant flow pump, and stirred for 12 hours at a temperature of 50°C, a pH value of 10.0, and a stirring rate of 500 rpm. After the solution reacted completely, it was filtered, washed, and dried to obtain manganese-based hydroxide Mn 0.75 Ni 0.25 (OH)2.
[0040] S2, weigh 11.2g of manganese-based hydroxide Mn prepared in step S1 0.75 Ni 0.25 (OH)2 and 5.8g sodium bicarbonate were added to 20mL ethanol and ball milled to mix evenly. After drying, a mixture was obtained. Under the condition of continuous air flow, the mixture was heated to 550℃ at a heating rate of 5℃ / min, kept warm for 6h, and cooled to obtain a sodium ion manganese-based precursor Na 0.4 Mn 0.75 Ni 0.25 O2.
[0041] S3. Weigh sodium carbonate at 0.3 times the sum of the amounts of manganese sulfate monohydrate and nickel sulfate hexahydrate in step S1, and then evenly mix the sodium carbonate and glucose with the sodium ion manganese-based precursor obtained in step S2 to obtain a mixture. Under nitrogen, add the mixture into a reactor containing deionized water and ethylene glycol (1:1) as a solvent, stir and react at 120° C. for 20 hours, and obtain a manganese-based sodium ion intermediate through filtration, washing, and drying.
[0042] S4, using the manganese-based sodium ion intermediate as the raw material, heating to 450 ° C at a heating rate of 5 ° C / min in a nitrogen atmosphere, keeping warm for 6 hours; then heating to 900 ° C at a heating rate of 5 ° C / min, calcining for 20 hours, and cooling naturally to obtain the sodium ion manganese-based positive electrode material Na 1.0 Mn 0.75 Ni 0.25 O2.
[0043] The XRD spectrum of the obtained sodium ion manganese-based positive electrode material is as follows Figure 1 As shown in the image, the structure of the obtained sodium ion manganese-based cathode material is a layered P2 phase Na 1.0 Mn 0.75 Ni 0.25 O2 structure.
[0044] The sodium ion manganese-based positive electrode material Na prepared in this embodiment 1.0 Mn 0.75 Ni 0.25 O2 is used as the positive active material for sodium ion battery preparation. The specific steps are:
[0045] Sodium ion manganese based cathode material Na 1.0 Mn 0.75 Ni 0.25 Sodium ion button batteries were prepared using O2 as the positive electrode active material, metallic sodium sheet as the negative electrode, and 1 mol / L NaPF6 and EC / DMC (volume ratio 1:1) as the electrolyte.
[0046] Then the battery's first charge and discharge curve, rate performance and cycle performance were tested, and the results were as follows: Figures 2-4 As shown. It is concluded that Na 1.0 Mn 0.75 Ni 0.25 O2 has a high first discharge capacity (158mAh / g); it has excellent rate performance, and under the condition of 5C (500mA / g) current charge and discharge, the discharge capacity can still reach 99.2mAh / g; it has good cycle performance, and the capacity retention rate reaches 99.4% after 100 charge and discharge cycles.
[0047] Example 2
[0048] A high specific capacity sodium ion manganese-based cathode material, its precursor and preparation method, comprising the following steps:
[0049] S1. Weigh 169.1 g of manganese sulfate monohydrate, 210.2 g of nickel sulfate hexahydrate, and 32.2 g of zinc sulfate, and add them to 1.0 L of water to prepare a mixed metal solution.
[0050] Add 160 g of sodium hydroxide and 23.5 mL of sodium sulfosalicylate (98%) to 1.0 L of water to obtain a sodium hydroxide mixed alkaline solution.
[0051] The mixed metal solution and the mixed alkali solution were added to the reactor simultaneously by a constant flow pump, and stirred for 12 hours at a temperature of 60°C, a pH value of 9.5, and a stirring rate of 500 rpm. After the solution reacted completely, it was filtered, washed, and dried to obtain manganese-based hydroxide Mn 0.5 Ni 0.4 Zn 0.1 (OH)2.
[0052] S2. Weigh 14.6 g of the manganese-based hydroxide obtained in step S1 and 5.8 g of sodium carbonate, add 20 mL of deionized water, and mix them by ball milling. After drying, a mixture is obtained.
[0053] Under the condition of continuous air flow, the mixture was heated to 550℃ at a heating rate of 5℃ / min, kept at this temperature for 6h, and cooled to obtain the sodium ion manganese-based precursor Na 0.43 Mn 0.5 Ni 0.4 Zn 0.1 O2.
[0054] S3, take 10g of sodium ion manganese-based precursor Na 0.43 Mn 0.5 Ni 0.4 Zn 0.1 O2, 3.2 grams of sodium carbonate and 0.48 grams of magnesium powder are added to the sodium ion manganese-based precursor, sodium carbonate and magnesium powder to obtain a mixture. Under nitrogen, the mixture is added into a reactor containing deionized water and triethanolamine (1:2) as a solvent, and the reaction is stirred at 80°C for 10 hours. The manganese-based sodium ion intermediate is obtained by filtration, washing and drying.
[0055] S4, using the manganese-based sodium ion intermediate as the raw material, heating to 450 ° C at a heating rate of 5 ° C / min in a nitrogen atmosphere, keeping warm for 6 hours; then heating to 900 ° C at a heating rate of 5 ° C / min, calcining for 20 hours, and cooling naturally to obtain the sodium ion manganese-based positive electrode material Na 0.92 Mn 0.48 Ni 0.38 Zn 0.096 Mg 0.044 O2.
[0056] The sodium ion manganese-based positive electrode material Na prepared in this embodiment 0.92 Mn 0.48 Ni 0.38 Zn 0.096 Mg 0.044 O2 is used as the positive active material for sodium ion battery preparation. The specific steps are:
[0057] Sodium ion manganese based cathode material Na 0.92 Mn 0.48 Ni 0.38 Zn 0.096 Mg 0.044 Sodium ion button batteries were prepared using O2 as the positive electrode active material, metallic sodium sheet as the negative electrode, and 1 mol / L NaPF6 and EC / DMC (volume ratio 1:1) as the electrolyte.
[0058] The battery's initial charge and discharge curve, rate performance, and cycle performance were then tested, and the results showed that the sodium-ion manganese-based positive electrode material had a high initial discharge capacity (161mAh / g); excellent rate performance, with a discharge capacity of up to 101mAh / g under 5C (500mA / g) current charge and discharge conditions; and good cycle performance, with a capacity retention rate of 98.6% after 100 charge and discharge cycles.
[0059] Example 3
[0060] A high specific capacity sodium ion manganese-based cathode material, its precursor and preparation method, comprising the following steps:
[0061] S1. Weigh 238.0 g of manganese sulfate monohydrate, 105.2 g of nickel sulfate hexahydrate, and 56.4 g of cobalt sulfate heptahydrate, and add them to 1.0 L of water to prepare a mixed metal solution.
[0062] 160 g of sodium hydroxide was added to 1.0 L of water to obtain a sodium hydroxide solution.
[0063] Then, the mixed metal solution, NaOH solution and 300 mL of 4% (mass fraction) ammonia water were added into the reactor simultaneously by a constant flow pump. Inert gas was introduced into the reactor for protection. The reaction was stirred for 12 hours at a temperature of 65 ° C, a pH value of 10.2 and a stirring rate of 300 rpm. After the solution reacted completely, it was filtered, washed and dried to obtain manganese-based hydroxide Mn 0.7 Ni 0.2 Co 0.1 (OH)2.
[0064] S2. Weigh 20 g of the manganese-based hydroxide obtained in step S1 and 6.5 g of sodium peroxide, add 30 mL of deionized water, and mix them by ball milling. After drying, a mixture is obtained.
[0065] Under the condition of continuous oxygen (purity 98%), the mixture was heated to 650℃ at a heating rate of 5℃ / min, kept at this temperature for 12h, and cooled to obtain the sodium ion manganese-based precursor Na 0.38 Mn 0.7 Ni 0.2 Co 0.1 O2.
[0066] S3, take 10g of sodium ion manganese-based precursor Na 0.38 Mn 0.7 Ni 0.2 Co 0.1 O2, 5.1 g of sodium bicarbonate and 0.78 g of sodium borohydride, and uniformly mix the sodium ion manganese-based precursor, sodium carbonate and sodium borohydride to obtain a mixture.
[0067] Under nitrogen atmosphere, the mixture was added into a reactor containing deionized water and NN-dimethylacetamide (1:5) as solvents, stirred and reacted at 150°C for 10 hours, and then filtered, washed, and dried to obtain a manganese-based sodium ion intermediate.
[0068] S4, using manganese-based sodium ion intermediate as raw material, in an argon atmosphere containing 10% hydrogen, heating to 550 ° C at a heating rate of 3 ° C / min, keeping warm for 6 hours; then heating to 900 ° C at a heating rate of 3 ° C / min, calcining for 24 hours, and cooling naturally to obtain sodium ion manganese-based positive electrode material Na 1.0 Mn 0.69 Ni 0.19 Co 0.1 B 0.02 O2.
[0069] The sodium ion-containing manganese-based positive electrode material prepared in this embodiment is used as the positive electrode active material for sodium ion batteries to prepare batteries. The specific steps are:
[0070] A lithium-ion button battery was prepared using sodium-ion manganese-based positive electrode material as the positive electrode active material, metallic sodium sheet as the negative electrode, and 1 mol / L NaPF6 and EC / DMC (volume ratio 1:1) as the electrolyte.
[0071] The battery's initial charge and discharge curve, rate performance, and cycle performance were tested, and it was concluded that the sodium-ion-containing lithium-rich manganese-based positive electrode material has a high initial discharge capacity (146 mAh / g); it has excellent rate performance, and under 5C (500 mA / g) current charge and discharge conditions, the discharge capacity can still reach 97 mAh / g; it has good cycle performance, and the capacity retention rate reaches 94.4% after 100 charge and discharge cycles.
[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solutions of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A manganese-based sodium ion positive electrode material, characterized in that: A manganese-based sodium ion intermediate is synthesized by a solvent thermal reduction method using a manganese-based precursor containing sodium ions as a raw material, and a manganese-based sodium ion intermediate is synthesized by high-temperature calcination using the manganese-based sodium ion intermediate as a raw material; The sodium ion-containing manganese-based precursor is prepared by embedding sodium ions into manganese-based hydroxide. The general formula of the sodium ion-containing manganese-based precursor is Na x Mn y M 1-y O z , 0< x ≤0.5, 0.5≤ y ≤1, 1≤ z ≤3; wherein M is any one or more of Ni, Co, Ti, Fe, Zn, Al, Cu, Nb, Ta, V, Cr, Sn, Si, Mo, W, Te, Mg, B, Zr, Y, and the valence of Mn is +4; The general formula of manganese-based sodium ion positive electrode material is Na n Mn y M 1-y O2, 0.5< n ≤1.5、0.5< y ≤1, where M is any one or more of Ni, Co, Ti, Fe, Zn, Al, Cu, Nb, Ta, V, Cr, Sn, Si, Mo, W, Te, Mg, B, Zr, and Y, and the valence of Mn is +3; A method for preparing a manganese-based sodium ion positive electrode material comprises the following steps: (1) According to the sodium ion-containing manganese-based positive electrode material Na n Mn y M 1-y O z Weigh a sodium source compound that is 0.5 to 1.5 times the sum of the amount of Mn and M in the solution, and then mix the sodium source compound, the reducing agent and the sodium ion-containing manganese-based precursor Na x Mn y M 1-y O z Mix well to obtain a mixture; (2) under the protection of an inert gas atmosphere, adding the mixture into a reaction kettle containing water and an organic reagent as solvents, reacting at a temperature of 50 to 300° C. for 1 to 48 hours, and filtering, washing, and drying to obtain a manganese-based sodium ion intermediate; (3) Using the manganese-based sodium ion intermediate as the raw material, heating to 200-500°C at a heating rate of 0.5-10°C / min under vacuum or inert atmosphere, and keeping warm for 2-30 hours; then heating to 600-1200°C at a heating rate of 0.5-10°C / min, calcining for 2-60 hours, and cooling to obtain the manganese-based sodium ion positive electrode material Na n Mn y M 1-y O2.
2. A manganese-based sodium ion positive electrode material according to claim 1, characterized in that: The preparation method of the sodium ion-containing manganese-based precursor comprises the following steps: S1, according to the general formula of the manganese-based precursor containing sodium ions Na x Mn y M 1-y O z Weigh a soluble salt of manganese element, a soluble compound containing M element or a soluble salt containing M metal element according to the stoichiometric ratio of the elements in the mixture, and add the soluble salt of manganese element and the soluble salt of M element into water to prepare a mixed solution; The mixed solution, precipitant solution and buffer solution are added into the reactor simultaneously by a constant flow pump, the reaction conditions are controlled to obtain a coprecipitate, and the precipitate is filtered, washed and dried. back To obtain manganese-based hydroxide; S2, according to the general formula of manganese-based precursor containing sodium ions Na x Mn y M 1-y O z The sum of the amounts of Mn and M in x times weighing a sodium source compound, and then evenly mixing the sodium source compound with the manganese-based hydroxide obtained in step S1 to obtain a mixture; Under the condition of continuous introduction of oxidizing gas, the mixture is heated to 200-800°C at a heating rate of 0.5-10°C / min, kept at this temperature for 1-48h, and cooled to obtain a sodium ion-containing manganese-based precursor Na x Mn y M 1-y O z ; In step S1, the soluble salt of manganese element is one or a combination of manganese chloride, manganese sulfate, manganese nitrate or manganese acetate; The buffer is one or a combination of ethylenediamine, ammonia water, hydroxylammonium hydrochloride, sodium sulfosalicylate, sodium phosphate, ethylenediaminetetraacetic acid, hydroxyethylethylenediaminetriacetic acid, ethylene glycol bis(2-aminoethyl ether)tetraacetic acid, diethyltriaminepentaacetic acid, and 1,2-cyclohexanediaminetetraacetic acid; the precipitant is sodium hydroxide; In step S2, the sodium source compound is one or a combination of sodium carbonate, sodium oxide, sodium peroxide, sodium hydroxide, sodium nitrate, sodium bicarbonate or sodium oxalate; Oxidizing gases are gases containing more than 10% oxygen or ozone.
3. A manganese-based sodium ion positive electrode material according to claim 1, characterized in that: In step (1), the sodium source compound is one or a combination of sodium carbonate, sodium oxide, sodium peroxide, sodium hydroxide, sodium nitrate, sodium bicarbonate or sodium oxalate.
4. The manganese-based sodium ion positive electrode material according to claim 1, characterized in that: In step (1), the reducing agent is one or a combination of ascorbic acid, glucose, sodium borohydride, sodium sulfite, sodium thiosulfate, magnesium, aluminum, zinc, tin, iron, oxalic acid, acetic acid, and aldehyde organic compounds.
5. The manganese-based sodium ion positive electrode material according to claim 1, characterized in that: In steps (2) and (3), the inert gas is one or a combination of several gases selected from nitrogen, argon, helium, hydrogen and carbon dioxide with a purity of more than 99%.