Positive electrode material of sodium ion battery as well as preparation method and application of positive electrode material
By adjusting the ratio of NaFePO4 and Na2FeP2O7 and organic carbon layer coating technology, the problem of impurities in the positive electrode material of sodium ion battery is solved, the electrochemical performance and energy density are improved, the discharge capacity is extended, and the low-cost and efficient sodium is achieved Preparation of positive electrode material for ion battery.
Patent Information
- Application Number
- CN202411117131.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
AI Technical Summary
The impurity NaFePO4 is present in the cathode materials of existing sodium ion batteries, which affects the electrochemical performance, and the preparation of pure phase materials is complex, resulting in insufficient energy density and cycle life.
By adjusting the ratio of NaFePO4 and Na2FeP2O7, the molecular composition of sodium ferric phosphate pyrophosphate is optimized, the heterophasic phase is reduced, the electrochemical potential of Fe2+/Fe3+ is increased, and the electrochemical potential is coated by an organic carbon layer to improve conductivity and mechanical strength.
The energy density and cycle life of the positive electrode material of sodium ion battery are achieved, the discharge capacity of more than 2.8V is extended, and the low-cost and non-toxic elements are used to simplify the preparation process.
Smart Images

Figure CN118993017A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a positive electrode material of a sodium ion battery and a preparation method and application thereof, belonging to the technical field of batteries. Background Art
[0002] With the development of the energy storage industry, the small storage amount of lithium (Li) element (20ppm) and its uneven distribution on the earth have seriously affected the development of the energy storage industry. Sodium (Na) is the fifth most abundant element in the earth's crust and has similar physical and chemical properties to Li. Sodium-ion batteries (SIBs) will become an ideal substitute for lithium-ion batteries in the future. Most of the technical difficulties currently faced by sodium-ion batteries are concentrated on the positive electrode materials. Sodium iron pyrophosphate Na4Fe3(PO4)2P2O7 (NFPP) has become one of the ideal choices for positive electrode materials for sodium-ion batteries due to its low cost, green environmental protection, good structural stability and long cycle life. However, due to the presence of a small amount of NaFePO4 impurities in Na4Fe3(PO4)2P2O7, the electrochemical properties of the material are affected, and the complex structure of Na4Fe3(PO4)2P2O7 has always been a major obstacle to the preparation of pure phase materials. Summary of the invention
[0003] To solve the above problems, the present invention provides a sodium iron pyrophosphate positive electrode material with reduced impurities, which is based on the optimization of Na4Fe3(PO4)2P2O7 with a current molecular configuration of 2.0NaFePO4:1.0Na2FeP2O7, and adjusts the ratio of NaFePO4 and Na2FeP2O7 to increase Fe 2+ / Fe 3+ electrochemical potential, extending the discharge capacity above 2.8V.
[0004] The first object of the present invention is to provide a method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0005] S1. Mix the sodium source, iron source, phosphorus source, organic carbon source and solvent according to the set ratio, and keep the pH at 6-8 during the mixing process;
[0006] S2, drying the mixture obtained in S1, and then heating it to a preset temperature for heat treatment to obtain the positive electrode material;
[0007] The molar ratio of sodium, iron, phosphate and pyrophosphate in the positive electrode material is (4-x+2y):(3-x+y):(2-x):(1+y), wherein 0<x<1, 0<y≤0.3.
[0008] Furthermore, in step S1, the set ratio is to first calculate the theoretical amount of each raw material according to the molar ratio, and the raw material containing phosphoric acid groups in the sodium source, iron source and phosphorus source exceeds the theoretical amount by 1wt% to 3wt%, and the raw material containing sodium element exceeds the theoretical amount by 1wt% to 5wt%.
[0009] Furthermore, the value range of x is 0<x<1, such as x=0.01, 0.02, 0.05, 0.07, 0.09, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.99, etc., including but not limited to the point values listed above.
[0010] Furthermore, the value range of y is 0<y≤0.3, such as y=0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, etc., including but not limited to the point values listed above.
[0011] Further, in step S1, the mixing includes at least one of the following:
[0012] (1) The mixing method includes ball milling;
[0013] (2) adjusting the slurry pH by adding a pH adjuster during the mixing process;
[0014] (3) The viscosity of the slurry during mixing is between 2000 and 4000 mPas;
[0015] (4) After the mixing process is completed, the particle size D90 of the slurry is less than 1 micron and / or the particle size D50 is 0.5-0.7 micron.
[0016] Furthermore, the pH adjuster includes phosphoric acid or sodium hydroxide.
[0017] Furthermore, in step S1, at least one of the following is included:
[0018] (1) The sodium source includes one or more of sodium-containing compounds such as sodium carbonate, sodium hydroxide, sodium dihydrogen phosphate, etc.;
[0019] (2) The iron source includes one or more of Fe-containing compounds such as ferric acetate monohydrate, ferric nitrate nonahydrate, ferrous oxalate monohydrate, ferric oxide, and ferric phosphate dihydrate;
[0020] (3) The phosphorus source includes one or more of phosphorus-containing compounds such as phosphoric acid, diammonium phosphate, diammonium hydrogen phosphate, and phosphorus pentoxide;
[0021] (4) The carbon source includes one or more of glucose, polyethylene glycol, citric acid, polyacrylic acid, lignin, cellulose, starch, polystyrene, polyvinyl pyrrolidone, polyacrylonitrile, etc.
[0022] Furthermore, in step S2, at least one of the following is included:
[0023] (1) The drying method includes spray drying;
[0024] (2) after the heat treatment, the mixture is further subjected to a grinding and screening step;
[0025] (3) The heating is carried out at a heating rate of 2-6°C per minute;
[0026] (4) The set temperature is 630° C.-670° C.;
[0027] (5) The heat treatment time is 5-10 hours.
[0028] Further, spray drying is performed at 100°C-150°C.
[0029] Furthermore, the particle size D50 after grinding and sieving is 5-10 microns.
[0030] Furthermore, the heating rate may include, but is not limited to, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, etc.
[0031] Further, the set temperature is such as 635℃, 640℃, 641℃, 642℃, 643℃, 644℃, 645℃, 646℃, 647℃, 648℃, 649℃, 650℃, 651℃, 652℃, 653℃, 654℃, 655℃, 656℃, 657℃, 658℃, 659℃, 660℃, 665℃, 670℃, including but not limited to the temperatures listed above.
[0032] Furthermore, the heat treatment time is such as 5.1h, 5.2h, 5.3h, 5.4h, 5.5h, 5.7h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 9.7h, 9.9h, etc., including but not limited to the time lengths listed above.
[0033] Further, in step S2, heat treatment is performed under a protective atmosphere, preferably an inert atmosphere.
[0034] A second object of the present invention is to provide a positive electrode material for a sodium ion battery, the positive electrode material comprising sodium ferric pyrophosphate and an organic carbon layer coated on the surface of the sodium ferric pyrophosphate;
[0035] The chemical formula of the sodium iron pyrophosphate is: (NaFePO4) 2-x (Na2FeP2O7) 1+y , where 0<x<1, 0<y≤0.3.
[0036] Another object of the present invention is to provide a positive electrode plate, comprising a current collector and a positive electrode active layer arranged on at least one side of the current collector along the thickness direction, wherein the positive electrode active layer comprises the positive electrode material of the above sodium ion battery or the positive electrode material prepared by the above preparation method.
[0037] Furthermore, the positive electrode active layer comprises the following components in mass percentage: 75-95% of positive electrode material, 5-15% of conductive agent and 5-15% of binder.
[0038] Furthermore, the conductive agent used in the present invention is selected from one or more of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0039] Further, the binder can be a binder well known to those skilled in the art without any particular limitation, such as chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacryloyl, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymer and guar gum copolymer. In the embodiment of the present invention, PVDF is selected.
[0040] Furthermore, the thickness of the positive electrode active layer ranges from 100 to 300 μm, for example, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, etc., including but not limited to the thickness values listed above.
[0041] The present invention also provides a method for preparing the positive electrode sheet as described above, comprising the following steps:
[0042] S01, preparing a positive electrode active slurry by using a formulated amount of positive electrode material, a conductive agent and a binder;
[0043] S02, coating the positive electrode active slurry on at least one side of the current collector along the thickness direction, obtaining a positive electrode active layer after drying, and pressing to obtain the positive electrode plate.
[0044] Furthermore, the current collector is aluminum foil, or other materials that can be used as a current collector; preferably, the thickness of the current collector is in the range of 5-14 μm.
[0045] The present invention also provides a sodium ion battery, comprising a negative electrode plate, a separator and an electrolyte, and importantly, comprising the positive electrode plate obtained above.
[0046] Furthermore, the negative electrode plate includes a negative electrode active layer; the negative electrode active layer includes a negative electrode active material, a conductive agent and a binder.
[0047] Furthermore, the negative electrode active layer comprises the following components in mass percentage: 75-95% of negative electrode active material, 5-15% of conductive agent and 5-15% of binder.
[0048] Furthermore, the negative electrode active material is selected from one or more of artificial graphite, natural graphite, silicon, silicon oxide, and sodium.
[0049] Furthermore, the conductive agent is selected from one or more of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0050] Furthermore, the binder can be a negative electrode binder well known to those skilled in the art without particular limitation, such as one or more of chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacryloyl, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymer and guar gum copolymer.
[0051] Furthermore, the type of the diaphragm can be any diaphragm familiar to those skilled in the art without any special restrictions, such as one or more of polyethylene, polypropylene, polyacrylonitrile, polyacrylonitrile fiber, polyamic acid, polyimide, polyamide, polydopamine, polyarylether sulfone, polyvinylidene fluoride, polyethylene oxide, polyethylene terephthalate, polyester, non-woven fabric membrane and cellulose paper-based isolation membrane.
[0052] Furthermore, the electrolyte can be any electrolyte well known to those skilled in the art without any special restrictions, the solvent is at least one of ethyl methyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate, dimethyl carbonate and diethylene glycol dimethanol ether; the electrolyte salt is at least one of sodium perchlorate, sodium bis(oxalate)borate, and sodium hexafluorophosphate.
[0053] Beneficial effects of the present invention:
[0054] In order to overcome the defect of many impurities in the current preparation process of sodium iron pyrophosphate, which affects the electrochemical performance, the present invention optimizes the ratio of NaFePO4 and Na2FeP2O7 at the same time, which becomes the key to improve the energy density of the positive electrode material. The elements used in the present invention are all low-cost and non-toxic elements, and the chemical formula of the prepared product can be expressed as: (NaFePO4) 2-x (Na2FeP2O7) 1+y / C (0<x<1, 0<y≤0.3), by adjusting the ratio of NaFePO4 and Na2FeP2O7 to increase the proportion of electronegative P2O7 groups, thereby increasing Fe 2+ / Fe 3+ The working potential can also extend the discharge capacity above 2.8V. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 (NaFePO4) prepared in Example 3 1.5 (Na2FeP2O7) 1.3 The first charge / discharge curves of the / C composite material at 0.1C rate when used as the positive electrode of sodium ion battery;
[0056] Figure 2 (NaFePO4) prepared in Example 3 1.5 (Na2FeP2O7) 1.3 TEM image of / C composites;
[0057] Figure 3 The first charge / discharge curve at a rate of 0.1C when the (NaFePO4)2(Na2FeP2O7) / C composite material prepared in Comparative Example 1 is used as a positive electrode of a sodium ion battery;
[0058] Figure 4 (NaFePO4) prepared in Comparative Example 2 2.0 (Na2FeP2O7) 1.4 The first charge / discharge curves of the / C composite material at 0.1C rate when used as the positive electrode of sodium ion battery;
[0059] Figure 5 (NaFePO4) prepared in Comparative Example 3 1.5 (Na2FeP2O7) 1.0 The first charge / discharge curves of the / C composite material at 0.1C rate when used as the positive electrode of sodium ion battery. DETAILED DESCRIPTION
[0060] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0061] The present invention provides a method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0062] S1. Mix the sodium source, iron source, phosphorus source, organic carbon source and solvent according to the set ratio, and keep the pH at 6-8 during the mixing process;
[0063] S2, drying the mixture obtained in S1, and then heating it to a preset temperature for heat treatment to obtain the positive electrode material;
[0064] The molar ratio of sodium, iron, phosphate and pyrophosphate in the positive electrode material is (4-x+2y): (3-x+y):
[0065] (2-x):(1+y), where 0<x<1, 0<y≤0.3.
[0066] Preferably, in step S1, the set ratio is to calculate the theoretical amount of each raw material in molar ratio, and the raw materials containing phosphate groups in the actually added sodium source, iron source and phosphorus source need to exceed the theoretical amount by 1wt% to 3wt%, and the raw materials containing sodium elements need to exceed the theoretical amount by 1wt% to 5wt%.
[0067] In the method, the raw materials containing phosphoric acid groups and sodium need to be appropriately excessive, which is due to normal losses during the preparation process and incomplete conversion. As experimentally verified, when the total excess ratio of raw materials containing phosphoric acid groups is between 1% and 3% and the total excess ratio of raw materials containing sodium elements is between 1wt% and 5wt%, the obtained material is closest to the theoretical target product, and the electrochemical performance after verification is also better. If the excess ratio is lower than this range, it will cause defects in cation sodium and anion PO4, thereby affecting the performance; if the excess ratio is higher than this range, it may be due to the incomplete reaction caused by the incorporation of additional cation sodium or anion PO4, resulting in an electrochemically inactive impurity phase (such as sodium phosphate, phosphate, etc.), reducing the specific capacity and average discharge voltage of the material.
[0068] Preferably, the value range of x is 0<x<1, such as x=0.01, 0.02, 0.05, 0.07, 0.09, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 0.99, etc., including but not limited to the point values listed above.
[0069] Preferably, the value range of y is 0<y≤0.3, such as y=0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, etc., including but not limited to the point values listed above.
[0070] Different from the traditional sodium ferric pyrophosphate with a molecular composition of 2.0NaFePO4:1.0Na2FeP2O7, the molecular composition of the sodium ferric pyrophosphate in the present invention is (2-x)NaFePO4:(1+y)Na2FeP2O7. Specifically, since NaFePO4 is considered to be a major impurity and has a great influence on the electrochemical performance, in order to obtain a pure phase, the present invention first reduces the amount of NaFePO4 in the synthesis stage, and adjusts the molar content of NaFePO4 in the sodium ferric pyrophosphate from 2 to 2-x (0<x<1). The characterization results show that when the content of NaFePO4 is reduced by a certain amount, the mixed anion-based compound may form a pure phase with a non-stoichiometric molecular formula, which provides a basis for reducing impurities. At the same time, the present invention also adjusts the content of Na2FeP2O7 in sodium iron pyrophosphate for the first time, and finds that a pure phase is formed when the content of Na2FeP2O7 is increased within a certain range, and it is verified that the electrochemical performance is further improved than when the Na2FeP2O7 content is not optimized, indicating that the new strategy of the present application has a reference significance for the pure phase synthesis of sodium iron pyrophosphate.
[0071] Preferably, in step S1, the mixing comprises at least one of the following:
[0072] (1) The mixing method includes ball milling;
[0073] (2) adjusting the slurry pH by adding a pH adjuster during the mixing process;
[0074] (3) The viscosity of the slurry during mixing is between 2000 and 4000 mPas;
[0075] (4) After the mixing process, the particle size D90 of the slurry is less than 1 micron and / or the particle size D50 is 0.5-0.7 micron.
[0076] Preferably, in step S1, the organic carbon source is soluble in the solvent.
[0077] Preferably, in step S1, the solvent selected includes but is not limited to organic solvents (such as ethanol, acetone, etc.), water, aqueous solutions, etc.
[0078] Wherein, the pH adjuster is preferably phosphoric acid or sodium hydroxide, which will not introduce new impurities.
[0079] Preferably, in step S1, at least one of the following is included:
[0080] (1) The sodium source includes one or more of sodium-containing compounds such as sodium carbonate, sodium hydroxide, sodium dihydrogen phosphate, etc.;
[0081] (2) The iron source includes one or more of Fe-containing compounds such as ferric acetate monohydrate, ferric nitrate nonahydrate, ferrous oxalate monohydrate, ferric oxide, and ferric phosphate dihydrate;
[0082] (3) The phosphorus source includes one or more of phosphorus-containing compounds such as phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphorus pentoxide;
[0083] (4) The carbon source includes one or more of glucose, polyethylene glycol, citric acid, polyacrylic acid, lignin, cellulose, starch, polystyrene, polyvinyl pyrrolidone, polyacrylonitrile, etc.
[0084] Preferably, in step S2, the drying method is preferably spray drying. Preferably, spray drying is performed at 100°C-150°C. The drying process of the present invention is performed after the mixing process, during which the organic carbon source is dissolved in the solvent and is evenly coated on the surface of the solid material when mixed with other raw materials, followed by spray drying and granulation, so that the organic carbon source is retained on the outer surface of other raw materials, ensuring that the organic carbon source in the final product forms a coating layer on the surface of sodium ferric phosphate pyrophosphate to obtain a core-shell structure.
[0085] Preferably, in step S2, the step of grinding the dried material is further included before heating, so as to facilitate uniform mixing of the raw materials and formation of a crystal structure in the subsequent sintering process.
[0086] Preferably, after the heat treatment in step S2, the method further comprises grinding and sieving the mixture. Most preferably, the particle size D50 after grinding and sieving is 5-10 microns.
[0087] The purpose of ball milling is to convert larger particles into smaller particles. After the powder particles are refined, the specific surface area of the material increases, which helps to improve the reaction rate and activity of the material. Therefore, in order to ensure the uniformity of material mixing and high reaction activity, the particle size D90 of the ball milling slurry is less than 1 micron, and the median particle size D50 is 0.5-0.7 micron; in order to increase the density of the powder obtained by spray drying in the subsequent process, the viscosity of the slurry needs to be maintained between 2000 and 4000mpas; the pH of the slurry during ball milling is 6-8. During the ball milling process, a pH adjuster such as phosphoric acid or sodium hydroxide can be added to adjust the pH to ensure that the iron source raw materials are in a stable state, no side reactions such as hydrolysis occur, and the slurry meets the requirements of particle size and viscosity.
[0088] Grinding and screening is to grind, crush and screen the sintered powder. The D50 of the secondary particle size after crushing is 5-10 microns, which is the balance between the electrode load and capacity. When the particle size is too large, the density of the powder is large, so the electrode load is high, but the capacity will be reduced; when the particle size is too small, the capacity of the powder is fully utilized, but the density of the powder is small, resulting in a small electrode load.
[0089] Preferably, in step S2, the temperature is increased at a heating rate of 2-6°C per minute. The heating rate is 2-6°C / min, such as 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, etc., including but not limited to the rates listed above.
[0090] Preferably, in step S2, the set temperature is 630°C-670°C, such as 635°C, 640°C, 641°C, 642°C, 643°C, 644°C, 645°C, 646°C, 647°C, 648°C, 649°C, 650°C, 651°C, 652°C, 653°C, 654°C, 655°C, 656°C, 657°C, 658°C, 659°C, 660°C, 665°C, 670°C, including but not limited to the temperatures listed above.
[0091] Preferably, in step S2, the heat treatment time is 5-10 hours, for example 5.1h, 5.2h, 5.3h, 5.4h, 5.5h, 5.7h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 9.7h, 9.9h, etc., including but not limited to the time lengths listed above.
[0092] The above appropriate sintering time and temperature promote the phosphate (PO4 3- ) and pyrophosphate (P2O7 4- ) is more completely converted, while the completely converted pyrophosphate (P2O7 4- ) has a higher electronegativity, thereby increasing the energy density.
[0093] The present invention also provides a positive electrode material for a sodium ion battery prepared by the above preparation method, wherein the positive electrode material comprises sodium ferric pyrophosphate and an organic carbon layer coated on the surface of the sodium ferric pyrophosphate;
[0094] The chemical formula of the sodium iron pyrophosphate is: (NaFePO4) 2-x (Na2FeP2O7) 1+y, 0<x<1, 0<y≤0.3, wherein: the molar ratio of sodium element, iron element, phosphate and pyrophosphate = (4-x+2y): (3-x+y): (2-x): (1+y).
[0095] As described in the background technology, the existing sodium iron pyrophosphate material usually contains impurities, and the presence of the impurities affects the application of the material. Therefore, technicians continue to explore the synthesis of the material in order to improve its electrochemical performance. The present invention not only controls the synthesis of NaFePO4, but also controls the synthesis of Na2FeP2O7. By simultaneously adjusting NaFePO4 and Na2FeP2O7, the ratio of the two is controlled within the range of (2-x): (1+y) (0<x<1, 0<y≤0.3). It has been verified that when the ratio of the two phases in the synthesized material falls within a specific range, the energy density of the positive electrode material is improved, and the specific capacity of the battery is greatly improved.
[0096] At the same time, the present invention designs the positive electrode material into a core-shell structure, the core layer is sodium ferric pyrophosphate with a specific structure, and the shell layer is an organic carbon layer. During the heat treatment process, the organic carbon source decomposes at a high temperature to form an amorphous carbon layer, which is uniformly attached to the surface of the material, which can not only promote the rapid conduction of electrons and improve the conductivity of sodium ferric pyrophosphate, but also the organic carbon layer can provide additional mechanical strength to protect the core material from environmental influences.
[0097] The present invention also provides a positive electrode plate, comprising a current collector and a positive electrode active layer arranged on at least one side of the current collector along the thickness direction, wherein the positive electrode active layer comprises the positive electrode material of the above sodium ion battery or the positive electrode material prepared by the above preparation method.
[0098] Preferably, the positive electrode active layer comprises the following components in mass percentage: 75-95% of positive electrode material, 5-15% of conductive agent and 5-15% of binder.
[0099] Preferably, the conductive agent used in the present invention is selected from one or more of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0100] Preferably, the binder is a binder well known to those skilled in the art, without any particular limitation, such as chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacryloyl, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymer and guar gum copolymer. In the embodiment of the present invention, PVDF is selected.
[0101] Preferably, the thickness of the positive electrode active layer is in the range of 100-300 μm, for example, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, etc., including but not limited to the thickness values listed above.
[0102] The present invention also provides a method for preparing the positive electrode sheet as described above, comprising the following steps:
[0103] S01, preparing a positive electrode active slurry by using a formulated amount of positive electrode material, a conductive agent and a binder;
[0104] S02, coating the positive electrode active slurry on at least one side of the current collector along the thickness direction, obtaining a positive electrode active layer after drying, and pressing to obtain the positive electrode plate.
[0105] Preferably, the current collector is aluminum foil, or other materials that can be used as a current collector; preferably, the thickness of the current collector is in the range of 5-14 μm.
[0106] The present invention also provides a sodium ion battery, comprising a negative electrode plate, a separator and an electrolyte, and importantly, comprising the positive electrode plate obtained above.
[0107] Preferably, the negative electrode plate comprises a negative electrode active layer; the negative electrode active layer comprises a negative electrode active material, a conductive agent and a binder.
[0108] Preferably, the negative electrode active layer comprises the following components in mass percentage: 75-95% of negative electrode active material, 5-15% of conductive agent and 5-15% of binder.
[0109] Preferably, the negative electrode active material is selected from one or more of artificial graphite, natural graphite, silicon, silicon oxide, and sodium.
[0110] Preferably, the conductive agent is selected from one or more of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0111] Preferably, the binder is a negative electrode binder well known to those skilled in the art without any particular limitation, such as one or more of chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacryloyl, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymer and guar gum copolymer.
[0112] Preferably, the type of the diaphragm is any diaphragm well known to those skilled in the art without any particular limitation, such as one or more of polyethylene, polypropylene, polyacrylonitrile, polyacrylonitrile fiber, polyamic acid, polyimide, polyamide, polydopamine, polyarylethersulfone, polyvinylidene fluoride, polyethylene oxide, polyethylene terephthalate, polyester, non-woven fabric membrane and cellulose paper-based isolation membrane.
[0113] Preferably, the electrolyte is an electrolyte well known to those skilled in the art without any special restrictions, the solvent is at least one of ethyl methyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate, dimethyl carbonate and diethylene glycol dimethanol ether; the electrolyte salt is at least one of sodium perchlorate, sodium bis(oxalate)borate, and sodium hexafluorophosphate.
[0114] Example 1
[0115] 16.3 g of sodium carbonate (1% excess), 54.4 g of ferric phosphate dihydrate, 16.1 g of sodium dihydrogen phosphate dihydrate (1% excess), 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of ionized water were mixed together and ball-milled. Phosphoric acid was added as a pH regulator during the process to maintain the pH of the slurry at 6-8 and the viscosity at 2000-4000 mpas. The slurry was ball-milled to a particle size of D90 = 0.951 μm and a median particle size of D50 = 0.55 μm. After ball-milling, the slurry was spray-dried at 120°C. The obtained powder was ground and then placed in a tubular atmosphere furnace for sintering at a heating rate of 5°C per minute, a sintering temperature of 650°C, and a holding time of 6 hours. The obtained powder was cooled and then ground and sieved to make the particle size D50 of 5-10 microns. The content of each metal element in the product was tested by inductively coupled plasma mass spectrometry (ICP-MS), and the content of phosphate and pyrophosphate was effectively separated and quantitatively analyzed by ion chromatography (the subsequent embodiments and comparative examples use the same method to determine the specific chemical formula of the obtained powder). According to the test record, it was confirmed by calculation that the final obtained was (NaFePO4) 1.9 (Na2FeP2O7) 1.01 / C composite material.
[0116] In the voltage range of 1.5~4.2V, the (NaFePO4) prepared in this example 1.9 (Na2FeP2O7) 1.01 The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. The material has 93.9mAh g at 0.1C (≥2.8V). -1 reversible discharge specific capacity.
[0117] Example 2
[0118] 14.45g sodium carbonate (1% excess), 54.4g ferric phosphate dihydrate, 17.2g sodium dihydrogen phosphate dihydrate (1% excess), 7.0g glucose, 1.7g polyethylene glycol and 120.0g ionized water were mixed together for ball milling. Phosphoric acid was added as a pH regulator during the process to maintain the pH of the slurry at 6-8, and the viscosity was maintained between 2000 and 4000mpas. The slurry was ball milled to a particle size of D90 = 0.9 microns and a median particle size of D50 = 0.6 microns. After ball milling, it was spray dried at 120°C. The obtained powder was ground and then placed in a tubular atmosphere furnace for sintering. The heating rate was 5°C per minute, the sintering temperature was 650°C, and the holding time was 6 hours. The obtained powder was cooled and then ground and sieved to make the particle size D50 5-10 microns. After testing and calculation, (NaFePO4) was finally obtained. 1.8 (Na2FeP2O7) 1.1 / C composite material.
[0119] In the voltage range of 1.5~4.2V, the (NaFePO4) prepared in this example 1.8 (Na2FeP2O7) 1.1 The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. The material has 94.4mAh g at 0.1C (≥2.8V). -1 reversible discharge specific capacity.
[0120] Example 3
[0121] 15.52g sodium carbonate (1% excess), 54.4g ferric phosphate dihydrate, 21.06g sodium dihydrogen phosphate dihydrate (1% excess), 7.0g glucose, 1.7g polyethylene glycol and 120.0g ionized water were mixed together for ball milling. Phosphoric acid was added as a pH regulator to keep the pH of the slurry at 6-8 and the viscosity at 2000-4000mpas. The slurry was ball milled to a particle size of D90 = 0.9 microns and a median particle size of D50 = 0.6 microns. After ball milling, the slurry was spray dried at 120°C. The obtained powder was ground and then placed in a tubular atmosphere furnace for sintering. The heating rate was 5°C per minute, the sintering temperature was 650°C, and the holding time was 6 hours. The obtained powder was cooled and then ground and sieved to make the particle size D50 5-10 microns. After testing and calculation, (NaFePO4) was finally obtained. 1.5 (Na2FeP2O7) 1.3 / C composite material.
[0122] In the voltage range of 1.5~4.2V, the (NaFePO4) prepared in this example 1.5 (Na2FeP2O7) 1.3The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. Figure 1 The charge / discharge curve at 0.1C rate shows that the material has a capacity of 94.6 mAh g at 0.1C (≥2.8 V). -1 reversible discharge specific capacity.
[0123] The prepared materials were tested by transmission electron microscopy (TEM). Figure 2 As shown, the outermost light-colored part is the carbon coating layer. The carbon coating layer is evenly coated and has a thickness of 2-5nm.
[0124] Example 4
[0125] 13.45g sodium hydroxide (2% excess), 41.61g ferric acetate monohydrate, 40.67g ammonium dihydrogen phosphate (2% excess), 7.0g glucose, 1.7g polyethylene glycol and 120.0g ionized water were mixed together for ball milling. Phosphoric acid was added as a pH regulator during the process to keep the pH of the slurry at 6-8 and the viscosity between 2000 and 4000mpas. The slurry was ball milled to a particle size of D90 = 0.98 microns and a median particle size of D50 = 0.7 microns. After ball milling, the slurry was spray dried at 150°C. The obtained powder was ground and then placed in a tubular atmosphere furnace for sintering. The heating rate was 6°C per minute, the sintering temperature was 630°C, and the holding time was 10 hours. The obtained powder was cooled and then ground and sieved to make the particle size D50 5-10 microns. After testing and calculation, (NaFePO4) was finally obtained. 1.1 (Na2FeP2O7) 1.2 / C composite material.
[0126] In the voltage range of 1.5~4.2V, the (NaFePO4) prepared in this example 1.1 (Na2FeP2O7) 1.2 The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. The material has 92.8mAh g at 0.1C (≥2.8V). -1 reversible discharge specific capacity.
[0127] Example 5
[0128] 12.98g sodium carbonate (3% excess), 98.98g ferric nitrate nonahydrate, 17.94g sodium dihydrogen phosphate monohydrate (3% excess), 7.0g glucose, 1.7g polyethylene glycol and 120.0g ionized water were mixed together for ball milling. Phosphoric acid was added as a pH regulator to keep the pH of the slurry at 6-8 and the viscosity at 2000-4000mpas. The slurry was ball milled to a particle size of D90 = 0.871 microns and a median particle size of D50 = 0.56 microns. After ball milling, the slurry was spray dried at 100°C. The obtained powder was ground and then placed in a tubular atmosphere furnace for sintering. The heating rate was 4°C per minute, the sintering temperature was 640°C, and the holding time was 8 hours. The obtained powder was cooled and then ground and sieved to make the particle size D50 5-10 microns. After testing and calculation, (NaFePO4) was finally obtained. 1.3 (Na2FeP2O7) 1.15 / C composite material.
[0129] In the voltage range of 1.5~4.2V, the (NaFePO4) prepared in this example 1.3 (Na2FeP2O7) 1.15 The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. The material has 93.1mAh g at 0.1C (≥2.8V). -1 reversible discharge specific capacity.
[0130] Example 6
[0131] 114.84g sodium carbonate (2% excess), 52.52g ferric phosphate dihydrate, 17.16g sodium dihydrogen phosphate monohydrate (1% excess), 7.0g glucose, 1.7g polyethylene glycol and 120.0g ionized water were mixed together for ball milling. During the process, a trace amount of sodium hydroxide was added as a pH regulator to keep the pH of the slurry at 6-8 and the viscosity at 2000-4000mpas. The slurry was ball milled to a particle size of D90 = 0.889 microns and a median particle size of D50 = 0.5 microns. After ball milling, it was spray dried at 130°C. The obtained powder was ground and then placed in a tubular atmosphere furnace for sintering. The heating rate was 3°C per minute, the sintering temperature was 670°C, and the holding time was 5 hours. The obtained powder was cooled and then ground and sieved to make the particle size D50 5-10 microns. After testing and calculation, (NaFePO4) was finally obtained. 1.7 (Na2FeP2O7) 1.1 / C composite material.
[0132] In the voltage range of 1.5~4.2V, the (NaFePO4) prepared in this example 1.7 (Na2FeP2O7) 1.1The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. The material has 93.7mAh g at 0.1C (≥2.8V). -1 reversible discharge specific capacity.
[0133] Comparative Example 1
[0134] 16.7 g of sodium carbonate (1% excess), 56.0 g of ferric phosphate dihydrate, 15.9 g of sodium dihydrogen phosphate dihydrate (1% excess), 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of ionized water were mixed together and ball milled. The remaining steps were the same as those in Example 3. After testing and calculation, the (NaFePO4)2(Na2FeP2O7) / C composite material was finally obtained.
[0135] In the voltage range of 1.5 to 4.2 V, a charge / discharge test was performed on a sodium ion battery using the (NaFePO4)2(Na2FeP2O7) / C composite material prepared in this comparative example as the positive electrode. Figure 3 The charge / discharge curve at 0.1C rate shows that the material has a capacity of 87.1 mAh g at 0.1C (≥2.8 V). -1 reversible discharge specific capacity.
[0136] Comparative Example 2
[0137] 18.02 g of sodium carbonate (1% excess), 63.77 g of ferric phosphate dihydrate, 21.84 g of sodium dihydrogen phosphate dihydrate (1% excess), 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of ionized water were mixed together for ball milling. The remaining steps were the same as those in Example 3. After testing and calculation, (NaFePO4) was finally obtained. 2.0 (Na2FeP2O7) 1.4 / C composite material.
[0138] In the voltage range of 1.5~4.2V, the prepared (NaFePO4) in this comparative example 2.0 (Na2FeP2O7) 1.4 The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. Figure 4 The charge / discharge curve at 0.1C rate shows that the material has a capacity of 82.6 mAh g at 0.1C (≥2.8 V). -1 reversible discharge specific capacity.
[0139] Comparative Example 3
[0140] 13.25 g of sodium carbonate (1% excess), 46.89 g of ferric phosphate dihydrate, 15.6 g of sodium dihydrogen phosphate dihydrate (1% excess), 7.0 g of glucose, 1.7 g of polyethylene glycol and 120.0 g of ionized water were mixed together for ball milling. The remaining steps were the same as those in Example 3. After testing and calculation, (NaFePO4) was finally obtained. 1.5 (Na2FeP2O7) 1.0 / C composite material.
[0141] In the voltage range of 1.5~4.2V, the prepared (NaFePO4) in this comparative example 1.5 (Na2FeP2O7) 1.0 The charge / discharge test of sodium ion battery with / C composite material as positive electrode was carried out. Figure 5 The charge / discharge curve at 0.1C rate shows that the material has a capacity of 72.3 mAh g at 0.1C (≥2.8 V). -1 reversible discharge specific capacity.
[0142] Comparative Example 4
[0143] No pH adjuster was added, and the pH was detected to be 9-10. The remaining steps were the same as those in Example 3 to obtain a composite material.
[0144] In the voltage range of 1.5 to 4.2 V, a sodium ion battery with the composite material prepared in this comparative example as the positive electrode was subjected to charge / discharge test. The material had a charge / discharge rate of 75.6 mAh g at 0.1 C (≥ 2.8 V). -1 reversible discharge specific capacity.
[0145] Comparative Example 5
[0146] First, the sodium source, iron source, phosphorus source and solvent are mixed, ball milled, spray dried, ground, and then sintered. The sintered product is ground and sieved, and a carbon source is added and sintered again to coat the carbon source on the surface. The specific steps are as follows:
[0147] 15.52g sodium carbonate (1% excess), 54.4g ferric phosphate dihydrate, 21.06g sodium dihydrogen phosphate dihydrate (1% excess) and 120.0g ionized water were mixed together for ball milling. Phosphoric acid was added as a pH regulator to keep the pH of the slurry at 6-8 and the viscosity at 2000-4000mpas. The slurry was ball milled to a particle size of D90 = 0.9 microns and a median particle size of D50 = 0.6 microns. After ball milling, the slurry was spray dried at 120°C. The obtained powder was ground and then placed in a tubular atmosphere furnace for sintering. The heating rate was 5°C per minute, the sintering temperature was 650°C, and the holding time was 6 hours. The product was ground and mixed with 7.0 g glucose, 1.7 g polyethylene glycol and 120.0 g ionized water, spray dried, sintered at 200-300°C to carbonize the organic carbon source, and the obtained powder was cooled and ground and sieved to obtain a particle size D50 of 5-10 μm to obtain (NaFePO4) 1.5 (Na2FeP2O7) 1.3 / C composite material.
[0148] In the voltage range of 1.5 to 4.2 V, a sodium ion battery using the composite material prepared in this comparative example as the positive electrode was subjected to charge / discharge tests. The material had a charge / discharge rate of 80.2 mAh g at 0.1 C (≥ 2.8 V). -1 reversible discharge specific capacity.
[0149] Test Example 1
[0150] Sodium ion batteries were constructed using the positive electrode materials prepared in the above embodiments and comparative examples, and the electrical properties of each battery were tested.
[0151] Preparation of sodium ion batteries
[0152] Positive electrode sheet: The positive electrode material prepared in the embodiment or comparative example, conductive carbon black (super P), and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 8:1:1, and N-methyl-2-pyrrolidone (NMP) was added and stirred to obtain a positive electrode active slurry. The positive electrode active slurry was evenly coated on the surface of the aluminum foil current collector, and a 200um blade coating was performed to prepare a pole sheet. After drying and cold pressing, a positive electrode sheet was obtained. The mass load of the active material was about 2.5 mg cm -2 .
[0153] Negative electrode: Sodium metal sheet.
[0154] Diaphragm: PE is selected as the isolation membrane with a thickness of 10μm.
[0155] Battery cell assembly: Arrange the positive electrode sheet, separator, negative electrode sheet and separator in sequence, and use winding as the assembly method.
[0156] Preparation of electrolyte: Sodium hexafluorophosphate is dissolved in ethylene carbonate at a concentration of 1 mol / L.
[0157] The electrolyte was injected into the dry battery cell, and after soaking for 24 hours, the battery cell was formed at 45°C. The formation process was as follows: charge at 0.05C to 3.4V, and then charge at 0.2C to 4.0V. After aging at room temperature for 24 hours, the battery cell was completed.
[0158] The results are as follows:
[0159] Table 1 Sodium ion battery related performance parameters
[0160]
[0161] As shown in Table 1, the first platform corresponds to Fe in NaFePO4 3+ / Fe 2+ The electrochemical conversion is the "sloping" part of the discharge curve (voltage> 2.9V), and the second platform corresponds to Fe in Na2FeP2O7. 3+ / Fe 2+ The electrochemical conversion is the "platform" part of the discharge platform (voltage is 2.8-2.9V). When prepared under the same conditions and when the content and ratio of phosphate (PO4) and pyrophosphate (P2O7) are different, the electrochemical performance of the corresponding battery is different. In Example 1, the ratio of phosphate to pyrophosphate is less than 2, and the electronegativity of P2O7 is stronger than that of PO4, which can improve Fe to a certain extent. 2+ / Fe 3+ The potential of the battery is increased. Increasing the proportion of P2O7 groups in NFPP helps to increase the discharge voltage of the battery. Example 2 and Example 3 As the content and ratio of phosphate and pyrophosphate change, the advantage of the electronegativity of P2O7 is brought into play, and the average discharge voltage of the material is improved. The capacity remains basically unchanged, and the battery energy density is improved. When the range of x and y is 0<x<1, 0<y≤0.3, on the one hand, Fe 2+ / Fe 3+ On the one hand, it is to ensure that a certain proportion of amorphous NaFePO4 is generated during the synthesis process, so as to ensure the capacity and the discharge medium voltage. By comparing the embodiments and comparative examples, it is found that when x≥1, the battery capacity is reduced (as shown in comparative example 1), and when y>0.3, both the specific capacity and the discharge medium voltage are reduced (as shown in comparative example 2). Compared with embodiment 3, comparative example 3 only reduces PO4 without increasing high electronegativity P2O7, although the ratio of phosphate to pyrophosphate is also less than 2, the average discharge voltage of the synthetic material is lower at this time.
[0162] In addition to the above-mentioned contents and proportions, the preparation process also affects the electrochemical properties of the obtained positive electrode material. Comparing Example 3 with Comparative Example 4, the only difference is whether the pH conditions in the preparation process are adjusted. When the pH value is not between 6-8, the iron source will be hydrolyzed to generate nano-scale iron hydroxide particles. At this time, the divalent iron ions will become trivalent iron ions, lose electrochemical activity, and cause a decrease in specific capacity. Compared with Comparative Example 5, the difference lies in the coating method of the organic carbon layer. In Example 3, a one-step method is adopted to mix other raw materials with the organic carbon source at the same time, and a composite material is obtained by ball milling, drying, and sintering in one step. In Comparative Example 5, a two-step method is adopted. After the NFPP particles are prepared, the organic carbon layer is coated. It is found that the positive electrode material prepared by the one-step method is better than the traditional two-step method. This not only simplifies the preparation method, but also achieves an improvement in the effect.
[0163] Test Example 2
[0164] Example 3 is used as a research basis to verify the influence of the addition amount of sodium source and phosphorus source on the performance of the synthetic material. In Example 3, sodium carbonate is used as a sodium element raw material in excess of 1%, and sodium dihydrogen phosphate dihydrate is used as a sodium element raw material and a PO4 group raw material in excess of 1%, so the total amount of sodium element raw materials is in excess of 2%, and the total amount of PO4 group raw materials is in excess of 1%. Of course, sodium dihydrogen phosphate dihydrate can also be directly used as a sodium element raw material and a PO4 group raw material to make the sodium source and the phosphorus source in excess of the same proportion.
[0165] Table 2 Effect of raw material addition on material properties
[0166]
[0167] A small amount of volatilization may occur in the sodium source during sintering, and the phosphorus source may have incomplete conversion of phosphate to pyrophosphate during the material synthesis process. Therefore, in the process of raw material matching, in order to ensure that the ideal compound is finally synthesized, the sodium source and phosphorus source need to be added in excess. This ensures that the loss of volatilization and incomplete conversion is fully taken into account during the synthesis process, so as to obtain the expected final product. When the sodium source and the phosphorus source are matched in the raw material ratio, there is no excess ratio or the excess ratio is insufficient (Example 3-2 and Example 3-3), which will cause the material to have cation sodium defects and anion PO4 defects, and the specific capacity and average discharge voltage of the material will decrease.
[0168] Based on Example 3, the effect of the particle size of ball milling and grinding and sieving on the performance of the synthetic material was verified. The results are shown in Table 3. As shown in Example 3-A, when the grinding and sieving particle size of the slurry cannot meet the corresponding standard, that is, the powder particle size in the slurry is too large, the powder with a larger particle size has a smaller specific surface area, resulting in a decrease in the contact area between the materials. This will affect the contact between the reactants, reduce the reaction rate, and prevent a complete reaction from occurring, resulting in the presence of trace impurities, thereby reducing the specific capacity. When the crushed particle size is greater than 10 microns, the specific capacity of the material is damaged due to the excessive ion transmission distance during the electrochemical reaction, as shown in Example 3-B; and when the crushed particle size is too small, as shown in Example 3-C, the specific capacity of the material is basically unchanged, but due to the decrease in compaction density, the specific energy of the battery is reduced.
[0169] Table 3 Effects of ball milling particle size and grinding and sieving particle size on material properties
[0170]
[0171] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A method for preparing a positive electrode material for a sodium ion battery, characterized in that: The following steps are involved: S1. Mix the sodium source, iron source, phosphorus source, organic carbon source and solvent according to the set ratio, and keep the pH at 6-8 during the mixing process; S2, drying the mixture obtained in S1, and then heating it to a preset temperature for heat treatment to obtain the positive electrode material; The molar ratio of sodium, iron, phosphate and pyrophosphate in the positive electrode material is (4-x+2y):(3-x+y):(2-x):(1+y), wherein 0<x<1, 0<y≤0.
3.
2. The preparation method according to claim 1, characterized in that: In step S1, the setting ratio is to first calculate the theoretical amount of each raw material according to the molar ratio, the raw material containing phosphoric acid groups in the sodium source, iron source and phosphorus source exceeds the theoretical amount by 1wt% to 3wt%, and the raw material containing sodium element exceeds the theoretical amount by 1wt% to 5wt%.
3. The preparation method according to claim 1, characterized in that: In step S1, the mixture includes at least one of the following features: (1) Mixing methods include ball milling; (2) adjusting the slurry pH by adding a pH adjuster during the mixing process; (3) The viscosity of the slurry during mixing is between 2000 and 4000 mPas; (4) After the mixing process is completed, the particle size D90 of the slurry is less than 1 micron and / or the particle size D50 is 0.5-0.7 micron.
4. The preparation method according to claim 3, characterized in that: The pH adjuster includes phosphoric acid or sodium hydroxide.
5. The preparation method according to claim 1, characterized in that: In step S1, at least one of the following features is included: (1) The sodium source includes one or more of sodium carbonate, sodium hydroxide, and sodium dihydrogen phosphate; (2) The iron source includes one or more of ferric acetate monohydrate, ferric nitrate nonahydrate, ferrous oxalate monohydrate, ferric oxide, and ferric phosphate dihydrate; (3) The phosphorus source includes one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphorus pentoxide; (4) The carbon source includes one or more of glucose, polyethylene glycol, citric acid, polyacrylic acid, lignin, cellulose, starch, polystyrene, polyvinyl pyrrolidone, and polyacrylonitrile; (5) The solvent includes one or more of an organic solvent, water, and an aqueous solution.
6. The preparation method according to claim 1, characterized in that: In step S2, at least one of the following features is included: (1) The drying method includes spray drying; (2) after the heat treatment, further comprising the step of grinding the mixture; (3) The heating is carried out at a heating rate of 2-6°C per minute; (4) The set temperature is 630° C.-670° C.; (5) The heat treatment time is 5-10 hours.
7. The preparation method according to claim 6, characterized in that: Contains at least one of the following characteristics: (1) spray drying at 100°C-150°C; (2) The particle size D50 after grinding is 5-10 microns.
8. A positive electrode material for a sodium ion battery, characterized in that: The positive electrode material includes sodium ferric pyrophosphate and an organic carbon layer coated on the surface of the sodium ferric pyrophosphate; The chemical formula of the sodium iron pyrophosphate is: (NaFePO4) 2-x (Na2FeP2O7) 1+y , where 0<x<1, 0<y≤0.
3.
9. A positive electrode sheet, comprising a current collector and a positive electrode active layer disposed on at least one side of the current collector along a thickness direction, characterized in that: The positive electrode active layer comprises the positive electrode material obtained by the preparation method according to any one of claims 1 to 7 or the positive electrode material according to claim 8.
10. A sodium ion battery, characterized in that: The sodium ion battery contains the positive electrode material obtained by the preparation method according to any one of claims 1 to 7, the positive electrode material according to claim 8, or the positive electrode sheet according to claim 9.
Citation Information
Patent Citations
Preparation method of water-based processing ferric sodium pyrophosphate
CN116986569A
Method for synthesizing nano polyanion sodium ion positive electrode material by soft template method
CN117776138A
Iron-based sodium pyrophosphate / C composite material and preparation and application thereof in sodium ion battery
CN118108202A
Preparation method of ferric sodium pyrophosphate and application of ferric sodium pyrophosphate in sodium ion battery
CN118439579A
Positive electrode active material and preparation method therefor, and positive electrode sheet, secondary battery and electric device comprising positive electrode active material
WO2024152193A1
Cited By
Na4Fe3 (PO4) 2 (P2O7) (at) C lithium ion battery positive electrode material, positive electrode and battery
CN119905549A
Preparation method and application of carbon shell coated ferric sodium pyrophosphate positive electrode material adaptive to aqueous binder
CN121020537A