A corrosion-resistant aluminum nitride ceramic substrate and preparation method thereof
By using carbon nickel-coated aluminum nitride powder and dibenzothiazole disulfide modification technology in aluminum nitride ceramic substrates, the problems of low bending strength and poor corrosion resistance of aluminum nitride ceramic substrates are solved, and their performance is significantly improved. Bending strength and corrosion resistance enhance the material's stability and application value.
Patent Information
- Application Number
- CN202411162234.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The current aluminum nitride ceramic substrate has low bending strength and poor corrosion resistance, which limits its application scope.
Using a combination of aluminum nitride powder, sintering aids, fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer, dispersant, plasticizer and solvent, the carbon nickel coating is formed through ball milling and sintering processes Aluminum nitride powder is surface modified using dibenzothiazole disulfide to improve sintering activity and density.
The bending strength and corrosion resistance of the aluminum nitride ceramic substrate are significantly improved, the bending strength loss rate due to acid corrosion is reduced, and the stability and application value of the material are enhanced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic substrates, and in particular to a corrosion-resistant aluminum nitride ceramic substrate and a preparation method thereof. Background Art
[0002] Aluminum nitride ceramic substrate is a new type of high-performance material made of aluminum nitride as the main component. Aluminum nitride is an inorganic compound with the characteristics of low thermal expansion coefficient, high hardness and excellent electrical properties. These characteristics make aluminum nitride ceramic substrates have a wide range of application value in many fields. Aluminum nitride ceramic substrates are widely used in the packaging, heat dissipation, insulation and support of electronic components. Due to its excellent thermal conductivity and insulation properties, it can effectively improve the working stability and reliability of components, so it is widely used in electronic products such as integrated circuits, power modules, sensors, etc. In the field of optoelectronics, aluminum nitride ceramic substrates are generally used to manufacture high-power LED packaging, laser packaging, optical fiber communication devices, etc. In addition, aluminum nitride ceramic substrates are also used in the manufacture of semiconductor manufacturing equipment, medical equipment, petrochemical equipment and other fields, and its application field is very wide.
[0003] Although aluminum nitride ceramic substrate is a high-performance material, it also has some defects. The current aluminum nitride ceramic substrate has poor mechanical properties. Although it has a certain hardness and mechanical strength, the bending strength of aluminum nitride ceramic is low under certain environments, which limits its application. In addition, the corrosion resistance of aluminum nitride ceramic substrate is poor, and its stability will be affected. Therefore, it is of great significance to develop an aluminum nitride ceramic substrate with high bending strength and good corrosion resistance. Summary of the invention
[0004] The invention provides a corrosion-resistant aluminum nitride ceramic substrate and a preparation method thereof, which solves the problems of low bending strength and poor corrosion resistance of the aluminum nitride ceramic substrate in the related art.
[0005] The technical solution of the present invention is as follows:
[0006] The present invention provides a corrosion-resistant aluminum nitride ceramic substrate, comprising the following raw materials in parts by weight:
[0007] 70-90 parts of aluminum nitride powder, 4-8 parts of sintering aid, 3-16 parts of fluorinated ethylene-propylene copolymer, 3-7 parts of stearic acid, 3-15 parts of ethylene-vinyl acetate copolymer, 1-3 parts of dispersant, 2-6 parts of plasticizer, and 60-70 parts of solvent.
[0008] As a further technical solution, the weight ratio of the fluorinated ethylene propylene copolymer, stearic acid and ethylene-vinyl acetate copolymer is 1~3:1:2.
[0009] When the weight ratio of the fluorinated ethylene propylene copolymer, stearic acid and ethylene-vinyl acetate copolymer is 1-3:1:2, the bending strength and corrosion resistance of the aluminum nitride ceramic substrate can be further improved.
[0010] As a further technical solution, the aluminum nitride powder is carbon-nickel coated aluminum nitride powder, and the components of the carbon-nickel coated aluminum nitride powder include aluminum nitride powder, graphite and nickel powder.
[0011] Graphite and nickel powder are coated on the aluminum nitride powder. The combination of graphite and nickel powder can improve the sintering activity of the aluminum nitride powder and improve the sintering efficiency, thereby promoting the densification of the aluminum nitride powder during the sintering process, and further improving the bending strength and corrosion resistance of the aluminum nitride ceramic substrate.
[0012] As a further technical solution, the weight ratio of the aluminum nitride powder, the graphite and the nickel powder is 14-18:1:1.
[0013] When the weight ratio of aluminum nitride powder, graphite and nickel powder is 14-18:1:1, the bending strength and corrosion resistance of the aluminum nitride ceramic substrate can be further improved.
[0014] As a further technical solution, the method for preparing the carbon-nickel coated aluminum nitride powder comprises the following steps: blending the aluminum nitride powder, the graphite and the nickel powder, and ball milling to obtain the carbon-nickel coated aluminum nitride powder.
[0015] As a further technical solution, during the ball milling, the rotation speed is 750-850 rpm and the time is 1-2 hours.
[0016] As a further technical solution, the particle size of the aluminum nitride powder is 2-10 μm, the particle size of the graphite is 30-500 nm, and the particle size of the nickel powder is 50-100 nm.
[0017] As a further technical solution, the carbon-nickel-coated aluminum nitride powder is dibenzothiazole disulfide-modified carbon-nickel-coated aluminum nitride powder; the preparation method of the dibenzothiazole disulfide-modified carbon-nickel-coated aluminum nitride powder includes the following steps: dissolving dibenzothiazole disulfide in dichloromethane to obtain a dibenzothiazole disulfide solution, adding carbon-nickel-coated aluminum nitride powder to the dibenzothiazole disulfide solution, dispersing evenly, and drying to obtain the dibenzothiazole disulfide-modified carbon-nickel-coated aluminum nitride powder.
[0018] The surface of the carbon-nickel coated aluminum nitride powder was modified by using dibenzothiazole disulfide. The sulfur element was introduced into the carbon-nickel coated aluminum nitride powder, which can further improve the sintering activity of the aluminum nitride powder, thereby further improving the bending strength and corrosion resistance of the aluminum nitride ceramic substrate.
[0019] As a further technical solution, the weight ratio of the carbon-nickel coated aluminum nitride powder to dibenzothiazole disulfide is 19-39:1.
[0020] When the weight ratio of carbon nickel coated aluminum nitride powder to dibenzothiazyl disulfide is 19-39:1, the bending strength and corrosion resistance of the aluminum nitride ceramic substrate can be further improved.
[0021] As a further technical solution, the mass fraction of the dibenzothiazyl disulfide solution is 2% to 8%.
[0022] As a further technical solution, the sintering aid is at least two of CaO, SiO2, TiO2, ZrO2, CaF2, and YCl3; the dispersant is one or more of castor oil, polymethacrylic acid, and polyethylene glycol stearate; the plasticizer is one or two of dibutyl phthalate and polyethylene glycol; the solvent is one or more of isopropanol, ethyl acetate, and anhydrous ethanol. Preferably, the sintering aid includes CaO and YCl3, and the weight ratio of CaO to YCl3 is 1:1.
[0023] The present invention also provides a method for preparing the corrosion-resistant aluminum nitride ceramic substrate, comprising the following steps:
[0024] S1. Except for the fluorinated ethylene-propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and plasticizer, the remaining raw materials in parts by weight are blended and ball-milled to obtain a mixture;
[0025] S2, adding fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and plasticizer to the mixture, mixing evenly to obtain a casting slurry;
[0026] S3, tape-casting the tape-casting slurry, drying, and punching to obtain a green body;
[0027] S4, debinding the green body and sintering it to obtain an aluminum nitride ceramic substrate.
[0028] As a further technical solution, in step S1, during the ball milling, the rotation speed is 700-800 rpm and the time is 5-10 hours; in step S4, during the sintering, the temperature is 1620-1720°C and the time is 2-5 hours.
[0029] The working principle and beneficial effects of the present invention are:
[0030] In the present invention, the raw materials of the aluminum nitride ceramic substrate include fluorinated ethylene propylene copolymer, stearic acid, and ethylene-vinyl acetate copolymer. The addition of fluorinated ethylene propylene copolymer, stearic acid, and ethylene-vinyl acetate copolymer can form a good dispersion system with aluminum nitride powder and sintering aid in the process of forming the casting slurry, so that the casting slurry is more uniform, thereby better shaping, and then in the sintering process, a more dense and stable aluminum nitride ceramic substrate is formed, which can significantly improve the bending strength and corrosion resistance of the aluminum nitride ceramic substrate. DETAILED DESCRIPTION
[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] In the following embodiments and comparative examples, the particle size of aluminum nitride powder is 5 μm; the particle size of graphite is 50 nm; the particle size of nickel powder is 80 nm; the model of fluorinated ethylene propylene copolymer is FJP-GD10; the model of ethylene-vinyl acetate copolymer is UL15019CC; the model of polymethacrylic acid is V020; and the model of polyethylene glycol is PEG-8000.
[0033] Example 1
[0034] A corrosion-resistant aluminum nitride ceramic substrate comprises the following raw materials in parts by weight:
[0035] 70 parts of aluminum nitride powder, 4 parts of sintering aids (2 parts of CaO and 2 parts of YCl3), 3 parts of fluorinated ethylene propylene copolymer, 3 parts of stearic acid, 3 parts of ethylene-vinyl acetate copolymer, 1 part of polymethacrylic acid, 2 parts of polyethylene glycol, 60 parts of isopropanol;
[0036] The preparation method thereof comprises the following steps:
[0037] S1, except the fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and polyethylene glycol, the remaining raw materials are blended by weight, and ball-milled at a rotation speed of 800 rpm for 5 hours to obtain a mixture;
[0038] S2, adding fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and polyethylene glycol to the mixture, mixing evenly to obtain a casting slurry;
[0039] S3, tape-casting the tape-casting slurry, drying, and punching to obtain a green body;
[0040] S4, debinding the green body, and sintering it at 1620° C. for 5 h to obtain an aluminum nitride ceramic substrate.
[0041] Example 2
[0042] A corrosion-resistant aluminum nitride ceramic substrate comprises the following raw materials in parts by weight:
[0043] 80 parts of aluminum nitride powder, 6 parts of sintering aids (3 parts of CaO and 3 parts of YCl3), 15 parts of fluorinated ethylene propylene copolymer, 3 parts of stearic acid, 6 parts of ethylene-vinyl acetate copolymer, 2 parts of polymethacrylic acid, 4 parts of polyethylene glycol, 65 parts of isopropanol;
[0044] The preparation method thereof comprises the following steps:
[0045] S1, except the fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and polyethylene glycol, the remaining raw materials are blended by weight, and ball-milled at a rotation speed of 750 rpm for 8 hours to obtain a mixture;
[0046] S2, adding fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and polyethylene glycol to the mixture, mixing evenly to obtain a casting slurry;
[0047] S3, tape-casting the tape-casting slurry, drying, and punching to obtain a green body;
[0048] S4, debinding the green body, and sintering it at 1670° C. for 3 h to obtain an aluminum nitride ceramic substrate.
[0049] Example 3
[0050] A corrosion-resistant aluminum nitride ceramic substrate comprises the following raw materials in parts by weight:
[0051] 90 parts of aluminum nitride powder, 8 parts of sintering aids (4 parts of CaO and 4 parts of YCl3), 16 parts of fluorinated ethylene propylene copolymer, 7 parts of stearic acid, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of polymethacrylic acid, 6 parts of polyethylene glycol, 70 parts of isopropanol;
[0052] The preparation method thereof comprises the following steps:
[0053] S1. Except for the fluorinated ethylene-propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and polyethylene glycol, the remaining raw materials are blended by weight, and ball-milled at a rotation speed of 700 rpm for 10 h to obtain a mixture;
[0054] S2, adding fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and polyethylene glycol to the mixture, mixing evenly to obtain a casting slurry;
[0055] S3, tape-casting the tape-casting slurry, drying, and punching to obtain a green body;
[0056] S4. Debinding the green body and sintering it at 1720° C. for 2 h to obtain an aluminum nitride ceramic substrate.
[0057] Example 4
[0058] The only difference between this embodiment and embodiment 2 is that in this embodiment, 4.5 parts of fluorinated ethylene propylene copolymer, 6.5 parts of stearic acid and 13 parts of ethylene-vinyl acetate copolymer are added.
[0059] Example 5
[0060] The only difference between this embodiment and embodiment 2 is that in this embodiment, 6 parts of fluorinated ethylene propylene copolymer, 6 parts of stearic acid and 12 parts of ethylene-vinyl acetate copolymer are added.
[0061] Example 6
[0062] The only difference between this embodiment and embodiment 2 is that in this embodiment, 12 parts of fluorinated ethylene propylene copolymer, 4 parts of stearic acid and 8 parts of ethylene-vinyl acetate copolymer are added.
[0063] Example 7
[0064] The only difference between this embodiment and embodiment 6 is that, in this embodiment, the aluminum nitride powder is carbon-coated aluminum nitride powder, and the preparation method of the carbon-coated aluminum nitride powder includes the following steps: blending 74 parts of aluminum nitride powder and 6 parts of graphite, and ball milling at a rotation speed of 800 rpm for 1.5 hours to obtain carbon-coated aluminum nitride powder.
[0065] Example 8
[0066] The only difference between this embodiment and embodiment 6 is that, in this embodiment, the aluminum nitride powder is nickel-coated aluminum nitride powder, and the preparation method of the nickel-coated aluminum nitride powder includes the following steps: blending 74 parts of aluminum nitride powder and 6 parts of nickel powder, and ball milling at a rotation speed of 800 rpm for 1.5 hours to obtain nickel-coated aluminum nitride powder.
[0067] Example 9
[0068] The only difference between this embodiment and embodiment 6 is that, in this embodiment, the aluminum nitride powder is carbon-nickel coated aluminum nitride powder, and the preparation method of the carbon-nickel coated aluminum nitride powder includes the following steps: 68 parts of aluminum nitride powder, 6 parts of graphite and 6 parts of nickel powder are blended, and ball milled at a rotation speed of 800 rpm for 1.5 hours to obtain carbon-nickel coated aluminum nitride powder.
[0069] Example 10
[0070] The only difference between this embodiment and embodiment 9 is that, in this embodiment, 74 parts of aluminum nitride powder, 3 parts of graphite, and 3 parts of nickel powder are added.
[0071] Embodiment 11
[0072] The only difference between this embodiment and embodiment 9 is that, in this embodiment, 70 parts of aluminum nitride powder, 5 parts of graphite, and 5 parts of nickel powder are added.
[0073] Example 12
[0074] The only difference between this embodiment and embodiment 9 is that, in this embodiment, 72 parts of aluminum nitride powder, 4 parts of graphite, and 4 parts of nickel powder are added.
[0075] Example 13
[0076] The only difference between this embodiment and embodiment 12 is that, in this embodiment, the carbon-nickel-coated aluminum nitride powder is dibenzothiazole disulfide-modified carbon-nickel-coated aluminum nitride powder, and the preparation method of dibenzothiazole disulfide-modified carbon-nickel-coated aluminum nitride powder comprises the following steps: dissolving 1 part of dibenzothiazole disulfide in dichloromethane to obtain a dibenzothiazole disulfide solution with a mass fraction of 2%, adding 79 parts of carbon-nickel-coated aluminum nitride powder (the weight ratio of aluminum nitride powder, graphite and nickel powder is 18:1:1) to the 2% dibenzothiazole disulfide solution, dispersing evenly, and drying to obtain dibenzothiazole disulfide-modified carbon-nickel-coated aluminum nitride powder.
[0077] Embodiment 14
[0078] The only difference between this embodiment and embodiment 13 is that in this embodiment, 74 parts of carbon-nickel-coated aluminum nitride powder are added (the weight ratio of aluminum nitride powder, graphite and nickel powder is 18:1:1), and 6 parts of dibenzothiazole disulfide are added.
[0079] Embodiment 15
[0080] The only difference between this embodiment and embodiment 13 is that in this embodiment, 76 parts of carbon-nickel-coated aluminum nitride powder are added (the weight ratio of aluminum nitride powder, graphite and nickel powder is 18:1:1), and 4 parts of dibenzothiazole disulfide are added.
[0081] Example 16
[0082] The only difference between this embodiment and embodiment 13 is that in this embodiment, 78 parts of carbon-nickel-coated aluminum nitride powder are added (the weight ratio of aluminum nitride powder, graphite and nickel powder is 18:1:1), and 2 parts of dibenzothiazole disulfide are added.
[0083] Comparative Example 1
[0084] The difference between this comparative example and Example 1 is that in this comparative example, no fluorinated ethylene propylene copolymer is added, 4.5 parts of stearic acid and 4.5 parts of ethylene-vinyl acetate copolymer are added.
[0085] Comparative Example 2
[0086] The difference between this comparative example and Example 1 is that in this comparative example, stearic acid is not added, 3 parts of fluorinated ethylene propylene copolymer and 6 parts of ethylene-vinyl acetate copolymer are added.
[0087] Comparative Example 3
[0088] The difference between this comparative example and Example 1 is that in this comparative example, no ethylene-vinyl acetate copolymer is added, 3 parts of fluorinated ethylene propylene copolymer are added, and 6 parts of stearic acid are added.
[0089] Comparative Example 4
[0090] The difference between this comparative example and Example 1 is that in this comparative example, no stearic acid and no ethylene-vinyl acetate copolymer are added, and 9 parts of fluorinated ethylene-propylene copolymer are added.
[0091] Comparative Example 5
[0092] The only difference between this comparative example and Example 1 is that in this comparative example, fluorinated ethylene propylene copolymer, stearic acid and ethylene-vinyl acetate copolymer are not added.
[0093] The following performance tests were performed on the aluminum nitride ceramic substrates prepared in Examples 1 to 16 and Comparative Examples 1 to 5:
[0094] Bending strength: According to the three-point bending test method of GB / T 6569-2006 "Test method for bending strength of fine ceramics", the bending strength of the aluminum nitride ceramic substrate sample was tested;
[0095] Corrosion resistance: After boiling the aluminum nitride ceramic substrate sample in a 20% sulfuric acid solution for 1 hour, the bending strength test after the acid corrosion test was carried out according to the above bending strength test method. The acid corrosion bending strength loss rate was calculated according to the following formula: acid corrosion bending strength loss rate = (bending strength before acid corrosion test - bending strength after acid corrosion test) / bending strength before acid corrosion test × 100%;
[0096] The test results are shown in Table 1 below:
[0097] Table 1 Test results
[0098]
[0099] Compared with Comparative Examples 1 to 5, the bending strength of Example 1 is significantly improved, and the acid corrosion bending strength loss rate is significantly reduced, indicating that when the raw materials of the aluminum nitride ceramic substrate include fluorinated ethylene propylene copolymer, stearic acid, and ethylene-vinyl acetate copolymer, the fluorinated ethylene propylene copolymer, stearic acid, and ethylene-vinyl acetate copolymer have a synergistic effect and can significantly improve the bending strength and corrosion resistance of the aluminum nitride ceramic substrate.
[0100] Compared with Examples 2 and 4, the bending strength of Examples 5 to 6 is improved, and the loss rate of bending strength in acid corrosion is reduced, indicating that when the weight ratio of fluorinated ethylene propylene copolymer, stearic acid and ethylene-vinyl acetate copolymer is 1 to 3: 1: 2, the bending strength and corrosion resistance of the aluminum nitride ceramic substrate can be further improved. Compared with Examples 6 to 8, the bending strength of Examples 9 to 12 is improved, and the loss rate of bending strength in acid corrosion is reduced, indicating that the bending strength and corrosion resistance of the aluminum nitride ceramic substrate can be further improved by coating the aluminum nitride powder with graphite and nickel powder. Compared with Examples 9 to 10, the bending strength of Examples 11 to 12 is improved, and the loss rate of bending strength in acid corrosion is reduced, indicating that when the weight ratio of aluminum nitride powder, graphite and nickel powder is 14 to 18: 1: 1, the bending strength and corrosion resistance of the aluminum nitride ceramic substrate can be further improved. Compared with Example 12, the bending strength of Examples 13 to 16 is improved, and the loss rate of bending strength by acid corrosion is reduced, indicating that the surface modification of the carbon-nickel-coated aluminum nitride powder by dibenzothiazole disulfide can further improve the bending strength and corrosion resistance of the aluminum nitride ceramic substrate. In addition, compared with Examples 13 to 14, the bending strength of Examples 15 to 16 is improved, and the loss rate of bending strength by acid corrosion is reduced, indicating that when the weight ratio of the carbon-nickel-coated aluminum nitride powder to dibenzothiazole disulfide is 19 to 39:1, the bending strength and corrosion resistance of the aluminum nitride ceramic substrate can be further improved.
[0101] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A corrosion-resistant aluminum nitride ceramic substrate, characterized in that: The invention comprises the following raw materials in parts by weight: 70-90 parts of aluminum nitride powder, 4-8 parts of sintering aid, 3-16 parts of fluorinated ethylene-propylene copolymer, 3-7 parts of stearic acid, 3-15 parts of ethylene-vinyl acetate copolymer, 1-3 parts of dispersant, 2-6 parts of plasticizer, and 60-70 parts of solvent; The aluminum nitride powder is carbon-nickel coated aluminum nitride powder, and the components of the carbon-nickel coated aluminum nitride powder include aluminum nitride powder, graphite and nickel powder; The carbon-nickel coated aluminum nitride powder is dibenzothiazole disulfide modified carbon-nickel coated aluminum nitride powder; the preparation method of the dibenzothiazole disulfide modified carbon-nickel coated aluminum nitride powder comprises the following steps: dissolving dibenzothiazole disulfide in dichloromethane to obtain a dibenzothiazole disulfide solution, adding carbon-nickel coated aluminum nitride powder to the dibenzothiazole disulfide solution, dispersing evenly, and drying to obtain the dibenzothiazole disulfide modified carbon-nickel coated aluminum nitride powder; The weight ratio of the carbon-nickel-coated aluminum nitride powder to dibenzothiazole disulfide is 19-39:
1.
2. The corrosion-resistant aluminum nitride ceramic substrate according to claim 1, characterized in that: The weight ratio of the fluorinated ethylene propylene copolymer, stearic acid and ethylene-vinyl acetate copolymer is 1-3:1:
2.
3. The corrosion-resistant aluminum nitride ceramic substrate according to claim 1, characterized in that: The weight ratio of the aluminum nitride powder, the graphite and the nickel powder is 14-18:1:
1.
4. The corrosion-resistant aluminum nitride ceramic substrate according to claim 1, characterized in that: The method for preparing the carbon-nickel coated aluminum nitride powder comprises the following steps: blending the aluminum nitride powder, the graphite and the nickel powder, and ball milling to obtain the carbon-nickel coated aluminum nitride powder.
5. The corrosion-resistant aluminum nitride ceramic substrate according to claim 1, characterized in that: The sintering aid is at least two of CaO, SiO2, TiO2, ZrO2, CaF2, and YCl3; the dispersant is one or more of castor oil, polymethacrylic acid, and polyethylene glycol stearate; the plasticizer is one or two of dibutyl phthalate and polyethylene glycol; and the solvent is one or more of isopropanol, ethyl acetate, and anhydrous ethanol.
6. The method for preparing a corrosion-resistant aluminum nitride ceramic substrate according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Except for the fluorinated ethylene-propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and plasticizer, the remaining raw materials in parts by weight are blended and ball-milled to obtain a mixture; S2, adding fluorinated ethylene propylene copolymer, stearic acid, ethylene-vinyl acetate copolymer and plasticizer to the mixture, mixing evenly to obtain a casting slurry; S3, tape-casting the tape-casting slurry, drying, and punching to obtain a green body; S4, debinding the green body and sintering it to obtain an aluminum nitride ceramic substrate.
7. The method for preparing a corrosion-resistant aluminum nitride ceramic substrate according to claim 6, characterized in that: In step S1, during the ball milling, the rotation speed is 700-800 rpm and the time is 5-10 hours; in step S4, during the sintering, the temperature is 1620-1720° C. and the time is 2-5 hours.
Citation Information
Patent Citations
Aluminium nitride-based multi-element nano-composite ceramic die material and preparation method thereof
CN104163632A
Nitride-based composite ceramic material for hydraulic steel pipe lining and preparation method of nitride-based composite ceramic material
CN106631077A
Cited By
Preparation method of high-toughness aluminum nitride substrate
CN119569474A