A highly antibacterial rare earth functional material and rare earth antibacterial fabric
By preparing the highly antibacterial rare earth functional material La@CN, combined with melt spinning technology, the problem of existing antibacterial fabrics being poor in preventing bacterial growth is solved, and effective inhibition and anti-mold effect on bacteria is achieved. It is suitable for a variety of textiles. Ensure human health and comfort.
Patent Information
- Application Number
- CN202411178836.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing antibacterial fabrics have limited effects in preventing bacterial growth and spread, especially in the microporous structure of textiles and the temperature and humidity environment of human body, bacteria are prone to reproduce and grow, leading to health threats.
Using the preparation method of highly antibacterial rare earth functional materials, the high antibacterial rare earth functional material La@ is obtained by reacting melamine, potassium permanganate and nano lanthanum oxide under oxygen atmosphere to form intermediate compounds and reacting with nitric acid under heating conditions. CN, combined with molten polypropylene terephthalate and vinyl triethoxysilane coupling agent for granulation and melt spinning, to prepare rare earth antibacterial fabrics.
By generating superoxide radicals and a stable crystal structure, this material significantly improves the antibacterial performance of a wide range of bacteria, especially the antibacterial effect of Gram-positive and negative bacteria, achieving an antibacterial rate of 99%, and is suitable for underwear, Textiles such as socks, towels and shoe linings ensure human health and comfort.
Smart Images

Figure CN118685878B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of fabrics, and in particular relates to a highly antibacterial rare earth functional material and a rare earth antibacterial fabric. Background Art
[0002] Bacteria are ubiquitous and widely distributed microorganisms in the human living environment. They are not only diverse, but also highly adaptable and reproduce very quickly. In particular, some harmful pathogens pose a serious threat to human health. They not only aggravate wound infection and disease progression through direct contact, but also indirectly invade the human body and cause disease by contaminating the surrounding environment (such as water, food, air, clothes, etc.).
[0003] Textiles and related products, as functional products essential to human life, are very easy to absorb and contaminate microorganisms due to their own microporous structure. In addition, the appropriate temperature and humidity on the human body surface, the secretion of oil and sweat, etc., create a favorable environment for the reproduction and growth of bacteria. Therefore, the development of functional textiles through rare earth materials has become a hot topic for researchers in this field.
[0004] There are four main technical approaches to the development of antibacterial fabrics: chemical modification technology, physical modification technology, spinning with antibacterial agents doped into spinning slurry, and composite spinning technology. In current production, spinning with antibacterial agents doped into spinning slurry to produce antibacterial yarns is the main means of developing antibacterial textiles.
[0005] Chemical grafting technology is to graft antibacterial groups onto the molecular chains of fiber macromolecules to make them antibacterial. Physical modification technology is to roughen and microporize the fiber surface, and add antibacterial agents into the spinning oil during the spinning process. When the fiber condenses and shrinks, the antibacterial agent is contained in the deeper part of the fiber surface and plays a role. Antibacterial agents are doped into the resin raw material for spinning. The main antibacterial agents used are mostly inorganic salts such as copper ions or silver ions. Composite spinning technology is to dope antibacterial agents into the fiber sheath layer to form core-sheath fibers, or as the parallel part of parallel fibers.
[0006] Rare earth materials play an important role in preventing infectious diseases and in the field of antibacterial treatment. A large number of studies have shown that rare earth ions have very strong broad-spectrum antibacterial properties. As long as enough rare earth ions are precipitated on the surface of the material, the material will have sufficient antibacterial efficiency, bacterial growth will be inhibited, and apoptosis will occur due to the destruction of the living environment. Summary of the invention
[0007] In view of this, the present invention aims to overcome the defects in the prior art and proposes a highly antibacterial rare earth functional material and a rare earth antibacterial fabric.
[0008] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0009] A method for preparing a highly antibacterial rare earth functional material comprises the following steps:
[0010] Step 1 is to add melamine, potassium permanganate and nano-lanthanum oxide into deionized water, heat it in an oxygen atmosphere, and stir it to obtain an intermediate compound;
[0011] Step 2 is to mix the intermediate compound with nitric acid and react under heating conditions to obtain a crude product;
[0012] Step 3 is to centrifuge and filter the crude product once to obtain a filter cake, disperse the filter cake in deionized water, perform ultrasonication, and centrifuge twice to obtain a precipitate;
[0013] Step 4 is to dry and calcine the precipitate to obtain the highly antibacterial rare earth functional material La@CN.
[0014] Furthermore, the mass ratio of melamine, potassium permanganate, nano-lanthanum oxide and deionized water in step 1 is 1:0.5-0.7:3.0-3.6; the temperature of the heating step in step 1 is 60-80°C; the stirring step in step 1 is magnetic stirring, and the time is 20-30 minutes.
[0015] Furthermore, the nano lanthanum oxide is prepared by a method comprising the following steps: dissolving lanthanum nitrate hexahydrate in deionized water, stirring to obtain a lanthanum nitrate solution, adding ammonia water and ammonium chloride solution to the deionized water, mixing evenly to obtain an ammonia water-ammonium chloride buffer solution, slowly adding the ammonia water-ammonium chloride buffer solution to the lanthanum nitrate solution to obtain a mixed solution, reacting the mixed solution under heating conditions, and obtaining the nano lanthanum oxide after centrifugation after the reaction is completed.
[0016] First, lanthanum nitrate La(NO3)3, as a precursor, undergoes hydrolysis in the solution. 3+ Ions and OH in water - ions combine to form La(OH)3. This is an acid-base neutralization reaction in which La 3+ As a Lewis acid, it accepts OH from water - ions. The La(OH)3 formed in the system is unstable during heating and easily decomposes to form La2O3. This step is achieved through heat treatment. The control of heat treatment temperature and time has an important influence on the particle size and morphology of the final product. Higher temperature promotes the growth of grains, while longer time contributes to the integrity and stability of the crystal form. Hydrothermal reaction is used to provide high temperature and high pressure conditions to obtain lanthanum oxide nanoparticles.
[0017] Furthermore, the mass ratio of the lanthanum nitrate hexahydrate to deionized water is 1:2.5-3.0; the mass concentration of the ammonia water is 10-25%, the mass concentration of the ammonium chloride solution is 10-25%, and the volume ratio of the ammonia water, the ammonium chloride solution and deionized water is 1:1-2:8-10; the temperature of the heating step is 180-220°C, and the reaction time is 10-12 hours; the rate of the centrifugation step is 8000-10000 rpm / 10 min.
[0018] Furthermore, the amount of nitric acid added in step 2 is 80-100% of the amount of melamine added, and the mass concentration of nitric acid is 10-37%; the temperature of the heating step in step 2 is 200-220° C.; and the time of the reaction step in step 2 is 6-8 hours.
[0019] Furthermore, the speed of the first centrifugation step in step 3 is 8000-10000 rpm / 10 min; the speed of the second centrifugation step in step 3 is 8000-10000 rpm / 10 min.
[0020] Furthermore, the temperature of the drying step in step 4 is 60-80° C. and the time is 12-18 h; the temperature of the calcining step in step 4 is 500-1200° C. and the time is 3-5 h.
[0021] A highly antibacterial rare earth functional material prepared by using the preparation method.
[0022] A method for preparing a rare earth antibacterial fabric comprises the following steps: granulating the highly antibacterial rare earth functional material, molten polytrimethylene terephthalate and vinyl triethoxysilane coupling agent to obtain solid particles, melt-spinning the solid particles to obtain spun fibers, stretching and heat-setting the spun fibers to obtain yarns, and weaving the yarns to obtain the rare earth antibacterial fabric; the mass ratio of the highly antibacterial rare earth functional material, molten polytrimethylene terephthalate and vinyl triethoxysilane coupling agent is 1:48-50:0.5-1.
[0023] A rare earth antibacterial fabric prepared by using the preparation method.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] The highly antibacterial rare earth functional material of the present invention uses nitrogen-containing compounds to prepare a carbon-nitrogen compound, which has a relatively rich lamellar structure after high-temperature calcination; and due to its own structure, the outer electrons combine with the oxygen on the surface of the material to generate superoxide free radicals, and further generate highly oxidizing hydroxyl free radicals; on the other hand, the rare earth material will be transformed into a stable crystalline structure after high-temperature calcination, and is a rare earth antibacterial material La@CN with strong antibacterial ability, which has very good effects on a wide range of Gram-positive bacteria and Gram-negative bacteria (tested by antibacterial experiments, it shows excellent antibacterial properties, and has good effects on common Gram-negative bacteria and Gram-positive bacteria such as Escherichia coli E. coli and Staphylococcus aureus S. aureus The antibacterial rate can reach 99%); Highly antibacterial rare earth functional materials combine the advantages of organic ligands and rare earth elements to produce a synergistic enhancement effect, further improving their antibacterial properties; when added to fabrics, they can effectively kill Escherichia coli and can be used in underwear, socks, towels and shoe linings. In daily life, they play an antibacterial and mildew-proof role, ensuring the comfort, safety and health of the human body.
[0026] The highly antibacterial rare earth functional material of the present invention can significantly improve the antibacterial performance of the fabric by being added to the fabric. According to the antibacterial test results, the antibacterial rate against Escherichia coli can reach 100%.
[0027] The particle size distribution of the highly antibacterial rare earth functional material of the present invention is between 120-170 nm, which can more effectively adapt to secondary processing and can also easily target and combine with pathogens to achieve an antibacterial effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The different rare earth antibacterial materials described in the embodiments of the present invention are E. coli Antibacterial evaluation effect diagram;
[0029] Figure 2 This is an XRD characterization test diagram of the rare earth antibacterial material La@CN described in an embodiment of the present invention;
[0030] Figure 3 This is a SEM environmental scanning electron microscope image of the rare earth antibacterial material La@CN described in an embodiment of the present invention: wherein, Figure A is 2 μm, and Figure B is 500 nm;
[0031] Figure 4 The La@CN rare earth antibacterial fabric described in the embodiment of the present invention is E. coli The antibacterial evaluation effect diagram: Figure A is the blank control, and Figure B is the rare earth antibacterial yarn;
[0032] Figure 5The rare earth antibacterial material described in the embodiment of the present invention adopts the antibacterial effect diagram of the modified nano lanthanum oxide of the present invention and the commercially available nano lanthanum oxide: wherein, Figure A is the commercially available nano lanthanum oxide, and Figure B is the homemade nano lanthanum oxide. DETAILED DESCRIPTION
[0033] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.
[0034] Melamine, nitric acid, sodium dihydrogen phosphate, potassium dihydrogen phosphate, lanthanum nitrate hexahydrate, vinyltriethoxysilane coupling agent (A151), sodium chloride, peptone, yeast extract, and agar were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0035] In addition, PBS buffer with a concentration of 0.03 mol / L and pH = 6.0 was prepared with distilled water using sodium dihydrogen phosphate and potassium dihydrogen phosphate as raw materials.
[0036] Escherichia coli ( E. coli ) was purchased from Guangdong Huankai Microbiology Technology Co., Ltd.
[0037] Staphylococcus aureus ( S. aureus ) was purchased from Guangdong Huankai Microbiology Technology Co., Ltd.
[0038] Polytrimethylene terephthalate (PTT) is produced by our partner China Textile Research Institute (Tianjin) Technology Development Co., Ltd.
[0039] The present invention will be described in detail below with reference to the embodiments.
[0040] Example 1
[0041] A method for preparing rare earth antibacterial fabric comprises the following steps:
[0042] (1) Weigh 375.82 g of lanthanum nitrate hexahydrate and dissolve it in 1.0 L of deionized water. Stir thoroughly to completely dissolve the lanthanum nitrate hexahydrate. Weigh 140 mL of 25% ammonia water and 140 mL of 25% ammonium chloride solution and add 1.1 L of deionized water. Stir evenly in a beaker to obtain an ammonia-ammonium chloride buffer solution. Slowly add the ammonia-ammonium chloride buffer solution to the lanthanum nitrate solution. Transfer the mixed solution to a hydrothermal reactor and react at 200°C for 12 h. After the reaction is completed, high-speed centrifugation (10,000 rpm / 10 min) is performed to remove excess unreacted impurities to obtain nano-lanthanum oxide.
[0043] (2) 100 g of melamine, 50 g of potassium permanganate and 320 g of nano-lanthanum oxide were added to 1 L of deionized water. An O2 balloon was connected to the top of the reactor and replaced repeatedly 3 times to ensure that the reaction was carried out in an O2 atmosphere. The temperature was then raised to 70 °C and stirred with external magnetic force for 30 min. The oxidation reaction caused some CN bonds in the carbon nitride sheet template to break, resulting in the loss of some atoms in the structure. The introduced rare earth ions could satisfy the charge balance of the defective parts, thereby obtaining a nano-two-dimensional sheet structure-intermediate compound. 45 mL of nitric acid was added to the intermediate compound, which was transferred into a hydrothermal reactor and reacted at 220 °C for 8 h to obtain a crude product. The crude product was collected by centrifugation (10000 rpm / 10 min) to precipitate, and was repeatedly filtered and washed three times with deionized water and anhydrous ethanol. The filter cake was dispersed in deionized water again and treated by ultrasound for 4 h, and then centrifuged again (10000 rpm / 10 min) collect the precipitate, dry it at 60°C, and then calcine it at 1200°C in a muffle furnace for 3 h to obtain a highly antibacterial rare earth functional material;
[0044] (3) 100 g of the highly antibacterial rare earth functional material, 4.8 kg of molten poly(trimethylene terephthalate) and 50 g of vinyl triethoxysilane coupling agent are added to a polyester granulator. The granulator compresses the polyester raw material and the rare earth additive into solid particles of uniform size and shape that meet the requirements through extrusion and friction. The solid particles are put into a spinning machine in batches. The solid particles are first melted by a heating device to obtain a spinning melt, and then the solid particles are quantitatively pressed out of the spinneret hole by a spinning pump through a screw continuous extruder, so that it is injected into the air in a thin stream and cooled in the spinning tunnel to form a filament. Then, the rare earth antibacterial yarn is obtained by winding the yarn roller, and finally, the yarn is interwoven together by a textile machine to form a fabric to obtain the rare earth antibacterial fabric.
[0045] Comparative Example 1
[0046] The only difference from Example 1 is that the nano-lanthanum oxide is a commercially available product (nano-lanthanum oxide was purchased from Shandong Mengxi New Materials Co., Ltd., D 50 is 50-200 nm. ).
[0047] The products obtained from Example 1 and each comparative example were tested as follows:
[0048] 1. Antibacterial test
[0049] 1. Preparation of culture medium:
[0050] Liquid LB medium: Add 10 g NaCl, 10 g tryptone, and 5 g yeast extract to 1 L pure water, stir evenly, and divide into 4 conical flasks. Sterilize in a high-pressure steam sterilizer at 121°C for 25 min before use.
[0051] Solid LB medium: add 10 g NaCl, 10 g tryptone, 5 g yeast extract and 15 g agar powder to 1 L pure water, sterilize at 121°C in a high pressure steam sterilizer for 25 min, then pour into a disposable culture dish while hot, wait for it to cool and solidify, seal with a sealing film and place in a 4°C refrigerator for later use.
[0052] 2. Escherichia coli ( E. coli )
[0053] Will buy E. coli After the freeze-dried powder and the resuscitation solution were mixed evenly, they were transferred to the LB culture medium prepared in advance and incubated in a constant temperature shaker for 6 h. Then, 500 μL of the second generation cultured cells were taken out in the clean bench. E. coli Then take 500 μL of 50% glycerol, mix well in a 2 mL EP tube, and store in a -80℃ refrigerator. E. coli The method of subculturing the strain is the same as that of the second generation.
[0054] 3. Effects of different rare earth antibacterial materials on E. coli Antibacterial performance test
[0055] First, freeze the third generation E. coli Transfer to the prepared LB culture medium, place in a constant temperature shaker and culture for 5 hours, then place in a clean bench E. coli The bacterial solution was diluted 104 times with PBS buffer, and then 10 mg of La@CN, 10 mg of Ce@CN, 10 mg of Gd@CN, and 10 mg of Y@CN were weighed and dissolved in 10 mL of PBS buffer and dispersed evenly with ultrasound. E. coli The bacterial solution and 100 μL of the prepared antibacterial material dispersion were mixed evenly and diluted to 1 mL with PBS buffer. A blank control experiment was performed at the same time. 100 μL of the diluted E. coli The bacterial solution was diluted to 1 mL with PBS buffer and incubated in a constant temperature shaker for 2 h.
[0056] After the incubation is completed, 100 μL of each sample is taken for plating. After 12 h of incubation in a constant temperature incubator, the growth of the colonies in the solid culture medium is as follows: Figure 1 shown.
[0057] The results showed that the blank culture medium without any antimicrobial agent was full of E. coli The number of single colonies in the culture medium with the addition of rare earth antibacterial materials was reduced, but only under the action of the La@CN antibacterial material prepared by the present invention, the number of colonies in the culture medium with the addition of rare earth antibacterial materials was reduced. E. coli The antibacterial rate is the best.
[0058] 2. XRD characterization test of rare earth antibacterial material La@CN
[0059] Based on the preliminary antibacterial performance evaluation of four modified rare earth materials, the antibacterial performance of La@CN material was screened out to be better than other materials. XRD characterization test of La@CN material was performed. Figure 2 shown.
[0060] The XRD diffraction spectrum of the La@CN sample shows that the product mainly contains two structures: lanthanum oxide and carbon nitride. Lanthanum oxide has a cubic fluorite structure and can still maintain a strong characteristic diffraction peak. The above results indicate that the rare earth element lanthanum reacts with the cyano group to form a stable coordination compound.
[0061] 3. SEM characterization test of rare earth antibacterial material La@CN
[0062] SEM scanning test of La@CN material Figure 3 shown.
[0063] from Figure 3 In the figure, we can see the overall structure with irregular distribution in the field of view. After magnifying the local morphology with 2 μm as the scale, we find that the large aggregates contain regular small-sized particles, ranging in size from about 200 to 800 nm. The different particle sizes come from the pseudo-agglomeration of the powder material during the calcination process, but the overall structure presents a relatively regular lamellar structure.
[0064] 4. La@CN rare earth antibacterial yarn E. coli Test
[0065] Weigh 0.75 g of each of the four rare earth antibacterial yarns, put them into a 50 mL conical flask and sterilize them in an autoclave at 121°C for 25 min before use. E. coli Transfer to the prepared LB culture medium, place in a constant temperature shaker and culture for 18 h, then place in a clean bench E. coli The bacterial solution was diluted 10 4 100 μL was then diluted to 10 in the clean bench. 4 times E. coliThe bacterial solution was added to a 50 mL conical flask and diluted to 10 mL with PBS buffer. It was then incubated in a constant temperature shaker for 6 h. After the incubation was completed, 100 μL of each sample was taken for plating. After 12 h of incubation in a constant temperature incubator, the growth of the colonies in the solid culture medium was as follows: Figure 4 shown.
[0066] The results showed that the blank yarn culture medium without any antimicrobial agent was full of E. coli The number of colonies in the culture medium of La@CN yarn with rare earth antibacterial materials was 0, which proved that La@CN yarn has strong antibacterial ability through melt spinning process. E. coli The antibacterial ability can reach 100%.
[0067] The antibacterial test of La@CN prepared by commercial nano-lanthanum oxide and the modified nano-lanthanum oxide of the present invention was carried out on the yarns made by melt spinning process. Figure 5 As shown, the antibacterial effect of the nano-lanthanum oxide of the present invention is significantly different from that of the La@CN yarn prepared by commercially available nano-lanthanum oxide.
[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a highly antibacterial rare earth functional material, characterized in that: The steps include: Step 1 is to add melamine, potassium permanganate and nano-lanthanum oxide into deionized water, heat it in an oxygen atmosphere, and stir it to obtain an intermediate compound; Step 2 is to mix the intermediate compound with nitric acid and react under heating conditions to obtain a crude product; Step 3 is to centrifuge and filter the crude product once to obtain a filter cake, disperse the filter cake in deionized water, perform ultrasonication, and centrifuge twice to obtain a precipitate; Step 4 is to dry and calcine the precipitate to obtain the highly antibacterial rare earth functional material La@CN; The nano lanthanum oxide is prepared by a method comprising the following steps: dissolving lanthanum nitrate hexahydrate in deionized water, stirring to obtain a lanthanum nitrate solution, adding ammonia water and ammonium chloride solution to the deionized water, mixing evenly to obtain an ammonia water-ammonium chloride buffer solution, slowly adding the ammonia water-ammonium chloride buffer solution to the lanthanum nitrate solution to obtain a mixed solution, reacting the mixed solution under heating conditions, and centrifuging to obtain the nano lanthanum oxide after the reaction is completed; The mass ratio of the lanthanum nitrate hexahydrate to deionized water is 1:2.5-3.0; the mass concentration of the ammonia water is 10-25%, the mass concentration of the ammonium chloride solution is 10-25%, and the volume ratio of the ammonia water, the ammonium chloride solution and the deionized water is 1:1-2:8-10; the temperature of the heating step is 180-220°C, and the reaction time is 10-12 hours; the speed of the centrifugation step is 8000-10000 rpm / 10 min; The calcination step in step 4 is performed at a temperature of 500-1200° C. and for a time of 3-5 h.
2. The method for preparing the highly antibacterial rare earth functional material according to claim 1, characterized in that: The mass ratio of melamine, potassium permanganate, nano-lanthanum oxide and deionized water in step 1 is 1:0.5-0.7:3.0-3.6; the temperature of the heating step in step 1 is 60-80° C.; the stirring step in step 1 is magnetic stirring, and the time is 20-30 minutes.
3. The method for preparing the highly antibacterial rare earth functional material according to claim 1, characterized in that: The amount of nitric acid added in step 2 is 80-100% of the amount of melamine added, and the mass concentration of nitric acid is 10-37%; the temperature of the heating step in step 2 is 200-220° C.; the time of the reaction step in step 2 is 6-8 hours.
4. The method for preparing the highly antibacterial rare earth functional material according to claim 1, characterized in that: The speed of the first centrifugation step in step 3 is 8000-10000 rpm / 10 min; the speed of the second centrifugation step in step 3 is 8000-10000 rpm / 10 min.
5. The method for preparing the highly antibacterial rare earth functional material according to claim 1, characterized in that: The temperature of the drying step in step 4 is 60-80° C. and the time is 12-18 h.
6. A highly antibacterial rare earth functional material prepared by the preparation method according to any one of claims 1 to 5.
7. A method for preparing rare earth antibacterial fabric, characterized in that: The method comprises the following steps: granulating the highly antibacterial rare earth functional material according to claim 6, molten polytrimethylene terephthalate and vinyl triethoxysilane coupling agent to obtain solid particles, melt-spinning the solid particles to obtain spun fibers, stretching and heat-setting the spun fibers to obtain yarns, and weaving the yarns to obtain the rare earth antibacterial fabrics; the mass ratio of the highly antibacterial rare earth functional material, molten polytrimethylene terephthalate and vinyl triethoxysilane coupling agent is 1:48-50:0.5-1.
8. A rare earth antibacterial fabric prepared by the preparation method according to claim 7.