A RTB series rare earth permanent magnet alloy flake and rare earth permanent magnet
By laser polishing, the problem of R-rich phase dispersion uniformity and cooling speed changes in R-T-B-based rare earth permanent magnets is solved, and the performance stability and magnetic properties of rare earth permanent magnets are improved, and a more uniform crystal structure and higher magnet properties.
Patent Information
- Application Number
- CN202411178251.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-27
AI Technical Summary
In the production of R-T-B rare earth permanent magnets, the dispersion uniformity of the R-rich phase is difficult to ensure, resulting in unstable magnet performance. The sandblasting method has hidden dangers of introducing external impurities and changes in cooling speed, which affects the uniformity of crystal structure.
The quench roller is treated with laser polishing to keep its roughness within a stable range, ensure the consistent cooling rate during casting, reduce the generation of ultrafine crystals and impurity phases, improve the uniform dispersion of R-rich phases and the crushing properties of rare earth permanent magnet alloy scales .
The performance stability and consistency of rare earth permanent magnets are achieved, defects in the smelting and powder making process are reduced, and the shrinkage ratio and magnetic properties of the magnet are improved.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of RTB-based rare earth material preparation, and relates to an RTB-based rare earth permanent magnet alloy flake and a rare earth permanent magnet, and in particular to an RTB-based rare earth permanent magnet alloy flake and an RTB-based rare earth permanent magnet prepared from the RTB-based rare earth permanent magnet alloy flake. Background Art
[0002] RTB rare earth permanent magnets are typical high-performance permanent magnets, where R represents at least one rare earth element, T represents at least one transition metal element, and B represents boron. In recent years, high-performance new energy vehicles have been continuously developed, among which high-performance permanent magnet motors are key components of new energy vehicles.
[0003] RTB rare earth permanent magnets are based on R2T 14 B is the main phase, and it has a rare earth element-rich, low-melting-point R-rich phase structure and a B-rich phase. RTB-based rare earth permanent magnets are usually prepared in the following way: first, the raw materials of the RTB-based rare earth permanent magnet alloy are mixed according to a ratio, melted, and alloy steel liquid is obtained, and rare earth alloy flakes are obtained by belt spinning. This process is generally carried out in a vacuum or inert gas atmosphere. The cast rare earth alloy flakes are made into alloy powder by hydrogen explosion and air flow milling, and then pressed into shape in a magnetic field, and sintered at a temperature of about 1000℃~1100℃ to obtain RTB-based rare earth permanent magnets; further, the obtained RTB-based rare earth permanent magnets will be heat treated and machined, and even surface treatments such as plating can be performed according to actual use requirements to improve corrosion resistance.
[0004] In RTB rare earth permanent magnets, the R-rich phase is the basic structure of RTB rare earth permanent magnets, which has a great influence on the performance of the magnets. It can improve the density and strength of the magnets, eliminate uneven grain boundaries, reduce the nucleation points of anti-magnetic domains, and isolate the main phase to improve the coercive force. If the R-rich phase is unevenly dispersed in the green body before sintering, the magnetization intensity and coercive force of the magnet will decrease. Therefore, ensuring the uniform dispersion of the R-rich phase and controlling the consistency of the uniform dispersion of the R-rich phase during the production process are the key points to obtain high-performance permanent magnets.
[0005] In order to ensure the consistency of the magnet production process, the industry often uses the method of sandblasting the periphery of the quench roller. However, the sandblasting method has the risk of introducing external impurities, and the surface state of the quench roller will change with the casting time during the casting process, resulting in changes in the cooling rate of the strip in the later stage of casting compared with the early stage of casting, and changes in the crystal structure deviation and uniformity of the crystal structure, which in turn leads to differences in the distribution of R-rich phase in the later stage of casting and the early stage of casting, resulting in poor dispersion uniformity and consistency of the R-rich phase in the production process of RTB rare earth alloy flakes.
[0006] In summary, there are still some problems in simply using the sandblasting method to ensure the uniformity of the R-rich phase dispersion to improve the magnet performance. Summary of the invention
[0007] In order to improve the problems existing in the prior art, the present invention provides an RTB-based rare earth permanent magnet alloy flake and an RTB-based rare earth permanent magnet. In the production process of the RTB-based rare earth permanent magnet alloy flake described in the present invention, the R-rich phase distribution has better stability, and the R-rich phase is more evenly dispersed, so that the RTB-based rare earth permanent magnet prepared by using the rare earth permanent magnet alloy flake has more stable shrinkage ratio and performance between different smelting furnaces during the production process, and better consistency. The crystal structure of the RTB-based rare earth permanent magnet is more uniform, which reduces the formation of ultrafine grains during the smelting process and the generation of transgranular fractures during the powder making process, and the performance of the RTB-based rare earth permanent magnet is higher.
[0008] The technical solution of the present invention is as follows:
[0009] An RTB-based rare earth permanent magnet alloy flake, the RTB-based rare earth permanent magnet alloy flake comprising two main surfaces and a plurality of columnar crystals radially extending from one main surface to the other main surface in the thickness direction;
[0010] The two main surfaces are the contact end surface of the quench roller and the free end surface opposite to the contact end surface of the quench roller; the thickness refers to the cross section perpendicular to the two main surfaces;
[0011] The columnar crystals satisfy: 0.9≤B1 / B2≤1.1;
[0012] Wherein, B1 is the average minor axis length of the columnar crystals located at the cross section perpendicular to the two main surfaces in the early stage of casting, in μm; B2 is the average minor axis length of the columnar crystals located at the cross section perpendicular to the two main surfaces in the later stage of casting, in μm;
[0013] The roughness of the chill roller satisfies: 0.9≤R1 / R2≤1.1;
[0014] Among them, R1 is the roughness of the surface of the quench roller in the early stage of casting, in μm; R2 is the roughness of the surface of the quench roller in the later stage of casting, in μm;
[0015] Among them, the first 1 / 3 of the casting time is the early casting period, and the last 1 / 3 of the casting time is the late casting period.
[0016] For example, if the casting time is 30 minutes, the first 10 minutes are the early casting period, and the last 10 minutes are the late casting period.
[0017] In the present invention, the two main surfaces refer to the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction, namely, the quench roller contact end surface and the free end surface opposite to the quench roller contact end surface.
[0018] According to an embodiment of the present invention, the quench roller contact end surface of the RTB rare earth alloy flake is the lower surface of the rare earth permanent magnet alloy flake along the length direction and the width direction, and the opposite surface that does not contact the quench roller is the free end surface, that is, the free end surface opposite to the quench roller contact end surface. The quench roller contact end surface is also called the roller contact surface, and the surface opposite to the quench roller contact end surface is called the free end surface.
[0019] According to an embodiment of the present invention, the cross section is the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flake along the length direction and the width direction; that is, the end face perpendicular to the roller surface and the free surface of the rare earth alloy flake is the cross section.
[0020] According to an embodiment of the present invention, B1 / B2 is 0.9, 0.95, 1.0, 1.05 or 1.1.
[0021] According to an embodiment of the present invention, R1 / R2 is 0.9, 0.95, 1.0, 1.05 or 1.1.
[0022] When the columnar crystal and roughness meet the above conditions respectively, the present invention has a relatively stable roughness of the quench roller in the early and late stages of casting, and obtains rare earth permanent magnet alloy flakes with a stable cooling rate and a more uniform crystal structure.
[0023] The present invention uses laser to continuously grind the quench roller during the casting process, so that the roughness of the quench roller is kept within a relatively stable range during the entire casting process, thereby ensuring that the cooling rate of the rare earth alloy flakes during the casting process is basically consistent, thereby maintaining the stability of the crystallization time and grain production time of the rare earth alloy flakes, and reducing the generation of coarse grains and a small amount of Fe-rich phases and other impurity phases in the late casting period. This helps to break the rare earth permanent magnet alloy flakes, enhance the stability of the powder making process, reduce the fluctuation of the shrinkage ratio of the green body during the sintering process, and is conducive to the control of the size and performance of the rare earth permanent magnet alloy during the production process.
[0024] According to an embodiment of the present invention, the plurality of columnar crystals satisfy: 2.0μm≤B1≤5μm; wherein B1 is the average short axis length of the plurality of columnar crystals in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the early stage of casting, in μm. Exemplarily, B1 is 2.0μm, 2.3μm, 2.5μm, 2.8μm, 3.0μm, 3.3μm, 3.5μm, 3.8μm, 4.0μm, 4.3μm, 4.5μm, 4.8μm or 5.0μm. B1 is obtained by testing, for example, by the following method: in the early stage of casting, on the contact end face of the quench roller, the number of columnar crystals per unit area is N, and the sum of the short axis lengths of the plurality of adjacent columnar crystals tested along the short axis direction of the columnar crystal is ∑B1, then the average short axis length of the columnar crystal on the contact end face of the quench roller is B1=∑B1 / N.
[0025] According to an embodiment of the present invention, the plurality of columnar crystals satisfy: 2.0 μm ≤ B1' ≤ 5 μm; wherein B1' is the short axis length of any columnar crystal in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the early stage of casting, in μm. Exemplarily, B1' is 2.0 μm, 2.3 μm, 2.5 μm, 2.8 μm, 3.0 μm, 3.3 μm, 3.5 μm, 3.8 μm, 4.0 μm, 4.3 μm, 4.5 μm, 4.8 μm or 5.0 μm.
[0026] According to an embodiment of the present invention, the plurality of columnar crystals satisfy: 2.0μm≤B2≤5μm; wherein B2 is the average short axis length of the plurality of columnar crystals in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the later stage of casting, in μm. Exemplarily, B2 is 2.0μm, 2.3μm, 2.5μm, 2.8μm, 3.0μm, 3.3μm, 3.5μm, 3.8μm, 4.0μm, 4.3μm, 4.5μm, 4.8μm or 5.0μm. B2 is obtained by testing, for example, by the following method: in the later stage of casting, on the contact end face of the quench roller, the number of columnar crystals per unit area is N, and the sum of the short axis lengths of the plurality of adjacent columnar crystals tested along the short axis direction of the columnar crystal is ∑B2, then the average short axis length of the columnar crystals on the contact end face of the quench roller is B2=∑B2 / N.
[0027] According to an embodiment of the present invention, the plurality of columnar crystals satisfy: 2.0 μm ≤ B2' ≤ 5 μm; wherein B2' is the short axis length of any columnar crystal in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the later stage of casting, in μm. Exemplarily, B2' is 2.0 μm, 2.3 μm, 2.5 μm, 2.8 μm, 3.0 μm, 3.3 μm, 3.5 μm, 3.8 μm, 4.0 μm, 4.3 μm, 4.5 μm, 4.8 μm or 5.0 μm.
[0028] According to an embodiment of the present invention, any columnar crystal satisfies: 2.0μm≤B1'≤5μm and 2.0μm≤B2'≤5μm. Studies have found that within this range, the R-rich phase can be more evenly distributed, easier to pulverize, easier to break during the airflow milling process, and can reduce the probability of transgranular fracture during the pulverization process, reduce the generation of crystal defects, and improve the performance of RTB-based rare earth permanent magnets. When the short axis length of the columnar crystal is greater than 5.0μm, the transgranular fracture of the rare earth permanent magnet alloy flakes increases during the powdering process, causing serious damage to the crystal structure of the RTB-based rare earth permanent magnet, causing the magnet performance to deteriorate or even fall below market demand; at the same time, it has a negative impact on the powdering process of the rare earth permanent magnet alloy flakes, for example, the difficulty of hydrogen explosion increases, the output of airflow milling decreases, and the production efficiency and magnets are greatly affected. When the short axis length of the columnar crystal is less than 2.0μm, a large number of ultrafine crystals will be generated in the rare earth permanent magnet alloy flakes. During the rare earth permanent magnet alloy flakes being crushed by air flow grinding, the ultrafine crystals will be converted into ultrafine powders and filtered out, and the ultrafine powders will usually be discarded, resulting in material waste. In addition, ultrafine crystals will also affect the mechanical strength and magnetic properties of the magnet.
[0029] According to an embodiment of the present invention, the roughness of the chill roller satisfies: 1μm≤R1≤20μm; wherein R1 is the roughness of the surface of the chill roller in the early stage of casting, in μm. Exemplarily, R1 is 1μm, 3μm, 5μm, 8μm, 10μm, 13μm, 15μm, 18μm or 20μm. R1 is obtained by, for example, the following method: in the early stage of casting, the roughness of N positions of the chill roller is tested using a roughness meter, and the roughness of each point is summed to obtain ∑R1, then the roughness in the early stage of casting R1=∑R1 / N.
[0030] According to an embodiment of the present invention, the roughness of the chill roller satisfies: 1μm≤R2≤20μm; wherein R2 is the roughness of the surface of the chill roller in the later stage of casting, in μm. Exemplarily, R2 is 1μm, 3μm, 5μm, 8μm, 10μm, 13μm, 15μm, 18μm or 20μm. R2 is obtained by testing, for example, by the following method: in the later stage of casting, the roughness of N positions of the chill roller is tested using a roughness meter, and the roughness of each point is summed to obtain ∑R2, then the roughness R2 in the later stage of casting = ∑R2 / N.
[0031] According to an embodiment of the present invention, the roughness of the quench roller satisfies: 1μm≤R1≤20μm and 1μm≤R2≤20μm. Studies have found that within this range, the cooling effect of the alloy steel liquid is better and more stable during the casting of rare earth permanent magnet alloy flakes, and the short axis length of the obtained columnar crystal meets the requirements and has better consistency. It can ensure that after the powder making process, the particle size distribution of the magnetic powder is more concentrated, the sintering process has a wider application range, the grain size in the final magnet is concentrated, and the grain boundary phase composition is more uniform, which is beneficial to improve the shrinkage ratio and stability of the permanent magnet and enhance the magnetic properties of the magnet.
[0032] According to an embodiment of the present invention, in the RTB rare earth permanent magnet alloy flakes, R is selected from at least one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb. In the preparation raw materials, the mass content of R is not less than 28wt% and not more than 35wt%; preferably not less than 29wt% and not more than 33wt%.
[0033] According to an embodiment of the present invention, in the RTB rare earth permanent magnet alloy flakes, T is selected from at least one or more of Co, Ga, Cu, Al, Nb, Zr, and Ti. In the preparation raw materials, the mass content of T is not less than 0.5wt% and not more than 5wt%; preferably not less than 1wt% and not more than 3wt%.
[0034] According to an embodiment of the present invention, in the raw material for preparing the RTB-based rare earth permanent magnet alloy flakes, the content of B is not less than 0.93wt% and not more than 1.3wt%; preferably not less than 0.95wt% and not more than 1.1wt%;
[0035] The rest is Fe and inevitable impurity elements.
[0036] The present invention also provides a method for preparing RTB-based rare earth permanent magnet alloy flakes, the method comprising:
[0037] (1) Mixing raw materials for preparing RTB series rare earth permanent magnet alloy flakes according to a proportion, melting them, and obtaining alloy steel liquid;
[0038] (2) Casting the alloy steel liquid of step (1) onto the surface of a rotating quench roller for a primary cooling treatment, and simultaneously performing laser treatment on the surface of the quench roller; then cooling the molten steel cast onto the surface of the quench roller and dropping it into a water-cooled drum for a secondary cooling treatment, and finally entering a cooling trolley for a tertiary cooling treatment, thereby preparing the RTB-based rare earth permanent magnet alloy flakes.
[0039] According to an embodiment of the present invention, in step (1), the raw materials for preparing the rare earth permanent magnet alloy flakes are not particularly defined, and can be raw materials for preparing rare earth permanent magnet alloy flakes known in the art. Specifically, the raw materials for preparing the rare earth permanent magnet alloy flakes can be selected according to the composition of the target RTB-based rare earth permanent magnet.
[0040] According to an embodiment of the present invention, in step (1), the melting temperature is 1200-1500° C., and the melting time (holding time after the raw materials are completely melted) is 5-60 min.
[0041] According to an embodiment of the present invention, in step (2), the rotation speed of the quench roller is ≥1.0 m / s, for example, 1.0-20 m / s; after the alloy steel liquid is cast onto the rotating quench roller surface, the alloy steel liquid will be cooled once on the quench roller surface.
[0042] According to an embodiment of the present invention, in step (2), circulating cooling water is introduced into the chill roller to ensure that the surface temperature of the chill roller is maintained at 10-50°C.
[0043] According to an embodiment of the present invention, in step (2), a laser is used to perform roughness treatment on the surface of the chill roller so that the roughness R of the chill roller is 1 to 20, in units of μm, and 0.9≤R1 / R2≤1.1, wherein R1 is the roughness of the surface of the chill roller in the early stage of casting, and R2 is the roughness of the surface of the chill roller in the later stage of casting.
[0044] According to an embodiment of the present invention, in step (2), the irradiation angle of the laser treatment is 20 to 80 degrees.
[0045] According to an embodiment of the present invention, in step (2), the irradiation speed of the laser treatment is 50-900 mm / sec.
[0046] According to the embodiment of the present invention, in step (2), the power energy density of the laser treatment is 0.5-50 GW / cm 2 .
[0047] According to an embodiment of the present invention, in step (2), the laser treatment is repeated 10 to 25 times.
[0048] According to an embodiment of the present invention, in step (2), the temperature of the cooling water in the water-cooling drum is 10-40°C.
[0049] According to an embodiment of the present invention, in step (2), the temperature of the cooling water of the cooling trolley is 10-60°C.
[0050] The present invention provides a rare earth permanent magnet alloy flake, and the rare earth permanent magnet alloy flake is prepared by the above method.
[0051] The present invention also provides an RTB series rare earth permanent magnet, which is prepared using the above-mentioned rare earth permanent magnet alloy flakes as raw materials.
[0052] The present invention also provides a method for preparing the above-mentioned RTB-based rare earth permanent magnet, the method comprising the following steps:
[0053] (a) grinding the rare earth permanent magnet alloy flakes through a jet mill after hydrogen explosion to obtain magnetic powder with a particle size range of 1-10 μm and an average particle size of 2.0-3.5 μm; adding an antioxidant to the magnetic powder and mixing them uniformly;
[0054] (b) pressing the magnetic powder of step (a) under a nitrogen atmosphere and a magnetic field greater than 1.8 T to obtain a green body;
[0055] (c) placing the green body of step (b) in a vacuum sintering furnace for sintering;
[0056] (d) subjecting the green body sintered in step (c) to a first-stage aging treatment and a second-stage aging treatment to obtain the RTB-based rare earth permanent magnet.
[0057] According to an embodiment of the present invention, in step (a), 0.02-5 wt% of an antioxidant (such as a fatty acid ester) is added to the magnetic powder, and mechanical stirring is continued for 3-6 hours until the magnetic powder is evenly dispersed.
[0058] According to an embodiment of the present invention, in step (b), the magnetic powder of step (a) is pressed and molded in a nitrogen atmosphere with a magnetic field strength of 2-5T and a magnetic field orientation direction.
[0059] According to an embodiment of the present invention, in step (b), the content of impurity elements in the green body satisfies: 100 ppm≤N content≤1400 ppm, 200 ppm≤H content≤3700 ppm.
[0060] Preferably, the content of the N element is 120 ppm, 200 ppm, 300 ppm, 400 ppm, 500 ppm, 800 ppm, 1000 ppm, 1200 ppm, 1300 ppm or 1400 ppm.
[0061] Preferably, the content of H element is 200 ppm, 300 ppm, 400 ppm, 500 ppm, 800 ppm, 1000 ppm, 1200 ppm, 1500 ppm, 1800 ppm, 2000 ppm, 2500 ppm, 3000 ppm, 3500 ppm or 3700 ppm.
[0062] According to an embodiment of the present invention, in step (c), the sintering treatment is to heat the temperature to 260-400°C (such as 260°C, 280°C, 300°C, 320°C, 350°C, 360°C, 380°C or 400°C) at a heating rate of 3-9°C / min, keep the temperature at 260-400°C for 40-70min (such as 40min, 50min, 60min or 70min), and then heat the temperature to 680-730°C (such as 680°C, 690°C) at a heating rate of 3-7°C / min. ℃, 700℃, 710℃, 720℃ or 730℃), keep it at 680-730℃ for 60-100min (such as 60min, 70min, 80min, 90min or 100min), then increase the temperature to 1050-1100℃ (such as 1050℃, 1060℃, 1070℃, 1080℃, 1090℃ or 1100℃) at a heating rate of 5-8℃ / min, and keep it at 1050-1100℃ for 3-6h (such as 3h, 4h, 5h or 6h).
[0063] According to an embodiment of the present invention, in step (c), the sintering process is performed under a vacuum environment.
[0064] According to an embodiment of the present invention, in step (c), the sintering treatment is followed by cooling to room temperature.
[0065] According to an embodiment of the present invention, in step (d), the temperature of the first aging treatment is 790-920°C (such as 790°C, 800°C, 820°C, 850°C, 860°C, 880°C, 900°C or 920°C), and the time of the first aging treatment is 3-6h (such as 3h, 4h, 5h or 6h); the temperature of the second aging treatment is 500-540°C (such as 500°C, 510°C, 520°C, 530°C or 540°C), and the time of the second aging treatment is 2-4h (such as 2h, 3h or 4h).
[0066] According to an embodiment of the present invention, in step (d), the first aging treatment is followed by cooling to room temperature, and then the temperature is continued to be raised for a second aging treatment.
[0067] The present invention also provides an RTB-based rare earth permanent magnet prepared by the method.
[0068] Beneficial effects of the present invention:
[0069] The present invention provides an RTB-based rare earth permanent magnet alloy flake, whose columnar crystals satisfy: 0.9≤B1 / B2≤1.1, and the roughness of the quench roller satisfies: 0.9≤R1 / R2≤1.1; when the columnar crystals and the roughness satisfy the above conditions respectively, the rare earth permanent magnet alloy flake of the present invention has a relatively stable quench roller roughness, cooling rate, and a more uniform crystal structure in the early and late stages of casting. Specifically, during the production process of the RTB-based rare earth permanent magnet alloy flake described in the present invention, the R-rich phase distribution has better stability, and the R-rich phase is more evenly dispersed, so that during the production process of the RTB-based rare earth permanent magnet prepared by using the rare earth permanent magnet alloy flake, the shrinkage ratio and performance between different smelting furnaces are more stable, and the consistency is better. The crystal structure of the RTB-based rare earth permanent magnet is more uniform, which reduces the formation of ultrafine crystals during the smelting process and the generation of transcrystalline fractures during the powder making process, and the performance of the RTB-based rare earth permanent magnet is higher.
[0070] The present invention adopts a laser grinding quench roller method to process the surface of the quench roller during the smelting and casting process, so that the roughness of the quench roller is kept within a relatively stable range, thereby ensuring that the thickness and cooling rate of the rare earth alloy flakes during the casting process are basically consistent, thereby maintaining the stability of the crystallization time and grain production time of the rare earth alloy flakes, and reducing the generation of coarse grains and a small amount of Fe-rich phases and other impurity phases in the late casting period. It is helpful to break the rare earth permanent magnet alloy flakes, enhance the stability of the powder making process, reduce the shrinkage ratio fluctuation of the green body during the sintering process, and is conducive to the control of the size and performance of the RTB series rare earth permanent magnet during the production process. DETAILED DESCRIPTION
[0071] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0072] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0073] The raw materials of NdFeB magnets in the embodiments and comparative examples of the present invention all adopt the same formula
[0074] Example 1
[0075] (1) The raw materials for preparing RTB rare earth permanent magnet alloy flakes are mixed according to the proportion, melted, and alloy steel liquid is obtained. The raw material proportion is: NdPr accounts for 31.1wt%, B accounts for 0.99wt%, Zr accounts for 0.18wt%, Ga accounts for 0.15wt%, Al accounts for 0.4wt%, Cu accounts for 0.15wt%, Co accounts for 1.52wt%, and the rest is Fe and unavoidable impurities, wherein the purity of each raw material is ≥99%. The melting temperature is 1450°C, and the melting time (holding time after the raw materials are completely melted) is 30min.
[0076] (2) The molten steel from step (1) is cast onto the surface of a rotating chill roller for primary cooling, and the surface of the chill roller is continuously laser polished; the molten steel cast onto the surface of the chill roller is then cooled and falls into a water-cooled drum for secondary cooling, and finally enters a cooling trolley for tertiary cooling. (3) In step (2), the rotation speed of the chill roller is 1.5 m / s.
[0077] In step (2), the cooling water temperature of the quench roller is 15°C.
[0078] In step (2), the roughness R1 of the chill roller is 8, in μm, and R1 / R2=0.98, where R1 is the surface roughness of the chill roller in the early stage of casting, and R2 is the roughness of the chill roller in the later stage of casting.
[0079] In step (2), the irradiation angle of the laser treatment is 25 degrees.
[0080] In step (2), the irradiation speed of the laser treatment is 100 mm / sec.
[0081] In step (2), the power energy density of the laser treatment is 10GW / cm2.
[0082] In step (2), the laser treatment is repeated 10 times.
[0083] Example 2
[0084] (1) Same as step (1) of Example 1.
[0085] (2) The molten steel of step (1) is cast onto the surface of a rotating quenching roller for a primary cooling treatment, and the surface of the quenching roller is continuously laser polished; the molten steel cast onto the surface of the quenching roller is then cooled and falls into a water-cooled drum for a secondary cooling treatment, and finally enters a cooling trolley for a tertiary cooling treatment.
[0086] (3) In step (2), the rotation speed of the cooling roller is 1.5 m / s.
[0087] In step (2), the cooling water temperature of the quench roller is 15°C
[0088] In step (2), the roughness R1 of the chill roller is 10, in μm, and R1 / R2=1.02, where R1 is the surface roughness of the chill roller in the early stage of casting, and R2 is the roughness of the chill roller in the later stage of casting.
[0089] In step (2), the irradiation angle of the laser treatment is 50 degrees.
[0090] In step (2), the irradiation speed of the laser treatment is 400 mm / sec.
[0091] In step (2), the power energy density of the laser treatment is 25GW / cm2.
[0092] In step (2), the laser treatment is repeated 15 times.
[0093] Example 3
[0094] (1) Same as step (1) of Example 1.
[0095] (2) The molten steel of step (1) is cast onto the surface of a rotating quenching roller for a primary cooling treatment, and the surface of the quenching roller is continuously laser polished; the molten steel cast onto the surface of the quenching roller is then cooled and falls into a water-cooled drum for a secondary cooling treatment, and finally enters a cooling trolley for a tertiary cooling treatment.
[0096] (3) In step (2), the rotation speed of the cooling roller is 1.5 m / s.
[0097] And / or, in step (2), the cooling water temperature of the quench roller is 15°C.
[0098] And / or, in step (2), the roughness R1 of the chill roller is 15, in μm, and R1 / R2=1, wherein R1 is the surface roughness of the chill roller in the early stage of casting, and R2 is the roughness of the chill roller in the later stage of casting.
[0099] And / or, in step (2), the irradiation angle of the laser treatment is 75 degrees.
[0100] And / or, in step (2), the irradiation speed of the laser treatment is 800 mm / sec
[0101] And / or, in step (2), the power energy density of the laser treatment is 42GW / cm 2 .
[0102] And / or, in step (2), the laser treatment is repeated 25 times.
[0103] Comparative Example 1
[0104] (1) Use 80-grit sandpaper to polish the cooling copper roller. The roughness R1 of the cooling roller is 2, and R1 / R2=1.38.
[0105] (2) The raw materials were melted and refined at a constant power of 550 kW; the raw materials were the same as those in step (1) of Example 1.
[0106] (3) The molten and refined steel is poured onto the polished cooling copper roller. The molten steel poured onto the surface of the quenching roller is then cooled once and falls into a water-cooled drum for secondary cooling, and finally enters a cooling trolley for tertiary cooling.
[0107] Comparative Example 2
[0108] (1) The cooling copper roller is sandblasted and polished using a sandblasting device. The sand material used for sandblasting is 10-mesh quartz sand. The roughness R1 of the cooling roller is 15, and R1 / R2=1.25.
[0109] (2) The raw materials were melted and refined at a constant power of 550 kW; the raw materials were the same as those in step (1) of Example 1.
[0110] (3) The molten and refined steel liquid is poured onto the polished cooling copper roller, and then the steel liquid cast onto the surface of the quenching roller is cooled once and falls into a water-cooled drum for secondary cooling, and finally enters a cooling trolley for tertiary cooling.
[0111] Comparative Example 3
[0112] (1) The cooling copper roller is sandblasted and polished using a sandblasting device. The sand material used in the sandblasting is 50 mesh steel sand. The roughness R1 of the cooling roller is 10, and R1 / R2=1.42.
[0113] (2) constant power melting and refining of raw materials at 550 kW;
[0114] (3) The molten and refined steel liquid is poured onto the polished cooling copper roller, and then the steel liquid cast onto the surface of the quenching roller is cooled once and falls into a water-cooled drum for secondary cooling, and finally enters a cooling trolley for tertiary cooling.
[0115] The scales prepared in the above-mentioned Examples 1-3 and Comparative Examples 1-3 are used to prepare rare earth permanent magnets. The specific preparation process of the rare earth permanent magnets refers to paragraphs 74-77 of the specification of patent CN117174420A, and the blank size and magnetic properties are tested.
[0116] After the cross-sections of the rare earth permanent magnet alloy flakes prepared in Examples 1-3 and Comparative Examples 1-3 were polished and corroded, a scanning electron microscope was used to observe the internal structure thereof; the width and length of the columnar crystals were measured using a 400x scanning electron microscope photograph field of view combined with a ruler.
[0117] The shrinkage ratio is calculated as blank size / pressed billet size. The ratio of the blank to pressed billet size in the three directions of product length, height, and orientation is the shrinkage ratio.
[0118] The test results are shown in Table 1.
[0119] Table 1
[0120] Initial scale thickness (mm) Later scale thickness mm B1 / B2 Br(T) Hcjka / m HK / Hcj Orientation shrinkage ratio Example 1 0.250 0.255 0.987 1.399 1472 0.985 0.680 Example 2 0.220 0.223 0.990 1.402 1487 0.997 0.679 Example 3 0.180 0.180 1.000 1.415 1500 0.992 0.676 Comparative Example 1 0.350 0.4 2.100 1.379 1393 0.975 0.695 Comparative Example 2 0.200 0.265 1.750 1.390 1421 0.982 0.685 Comparative Example 3 0.230 0.300 1.703 1.383 1430 0.980 0.683
[0121] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An RTB rare earth permanent magnet alloy flake, characterized in that: The RTB rare earth permanent magnet alloy flakes include two main surfaces and a plurality of columnar crystals extending radially from one main surface to the other main surface in the thickness direction; The two main surfaces are the contact end surface of the quench roller and the free end surface opposite to the contact end surface of the quench roller; the thickness refers to the cross section perpendicular to the two main surfaces; The columnar crystals satisfy: 0.9≤B1 / B2≤1.1; Wherein, B1 is the average minor axis length of the columnar crystals located at the cross section perpendicular to the two main surfaces in the early stage of casting, in μm; B2 is the average minor axis length of the columnar crystals located at the cross section perpendicular to the two main surfaces in the later stage of casting, in μm; The roughness of the chill roller satisfies: 0.9≤R1 / R2≤1.1; Among them, R1 is the roughness of the surface of the quench roller in the early stage of casting, in μm; R2 is the roughness of the surface of the quench roller in the later stage of casting, in μm; Among them, the first 1 / 3 of the casting time is the early casting period, and the last 1 / 3 of the casting time is the late casting period; 1μm≤R1≤20μm; 1μm≤R2≤20μm.
2. The alloy flake according to claim 1, characterized in that: The plurality of columnar crystals satisfy: 2.0 μm≤B1≤5 μm; wherein B1 is the average minor axis length of the plurality of columnar crystals in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the early stage of casting, in μm; And / or, the plurality of columnar crystals satisfy: 2.0 μm≤B1′≤5 μm; wherein B1′ is the minor axis length of any columnar crystal in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the early stage of casting, in μm.
3. The alloy flake according to claim 1, characterized in that: The plurality of columnar crystals satisfy: 2.0 μm ≤ B2 ≤ 5 μm; wherein B2 is the average minor axis length of the plurality of columnar crystals in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the later stage of casting, in μm; And / or, the plurality of columnar crystals satisfy: 2.0 μm≤B2'≤5 μm; wherein B2' is the minor axis length of any columnar crystal in the cross section of the upper and lower surfaces of the rare earth permanent magnet alloy flakes along the length direction and the width direction in the later stage of casting, in μm.
4. The method for preparing the RTB-based rare earth permanent magnet alloy flakes according to any one of claims 1 to 3, characterized in that: The method comprises: (1) Mixing raw materials for preparing RTB series rare earth permanent magnet alloy flakes according to a proportion, melting them, and obtaining alloy steel liquid; (2) Casting the alloy steel liquid of step (1) onto the surface of a rotating quench roller for a primary cooling treatment, and simultaneously performing laser treatment on the surface of the quench roller; then cooling the molten steel cast onto the surface of the quench roller and dropping it into a water-cooled drum for a secondary cooling treatment, and finally entering a cooling trolley for a tertiary cooling treatment, thereby preparing the RTB-based rare earth permanent magnet alloy flakes.
5. The method according to claim 4, characterized in that In step (2), the rotation speed of the cooling roller is ≥1.0 m / s.
6. The method according to claim 4, characterized in that In step (2), the surface of the chill roller is roughened by laser so that the roughness R of the chill roller is 1-20, in μm, and 0.9≤R1 / R2≤1.1, where R1 is the roughness of the chill roller surface in the early stage of casting, and R2 is the roughness of the chill roller surface in the later stage of casting.
7. The method according to claim 4, characterized in that In step (2), the irradiation angle of the laser treatment is 20 degrees to 80 degrees; and / or, in step (2), the irradiation speed of the laser treatment is 50 to 900 mm / sec; And / or, in step (2), the power energy density of the laser treatment is 0.5~50GW / cm 2 ; And / or, in step (2), the laser treatment is repeated 10 to 25 times.
8. An RTB rare earth permanent magnet, characterized in that: The RTB series rare earth permanent magnet is prepared using the rare earth permanent magnet alloy flakes described in any one of claims 1 to 3 or the rare earth permanent magnet alloy flakes prepared by the method described in any one of claims 5 to 7 as raw materials.
9. The method for preparing the RTB-based rare earth permanent magnet according to claim 8, comprising the following steps: (a) grinding the rare earth permanent magnet alloy flakes through a jet mill after hydrogen explosion to obtain magnetic powder with a particle size range of 1-10 μm and an average particle size of 2.0-3.5 μm; adding an antioxidant to the magnetic powder and mixing them uniformly; (b) pressing the magnetic powder of step (a) under a nitrogen atmosphere and a magnetic field greater than 1.8 T to obtain a green body; (c) placing the green body of step (b) in a vacuum sintering furnace for sintering; (d) subjecting the green body sintered in step (c) to a first-stage aging treatment and a second-stage aging treatment to obtain the RTB-based rare earth permanent magnet.
10. The RTB rare earth permanent magnet prepared by the method according to claim 9.
Citation Information
Patent Citations
Rare earth permanent magnet alloy scale and neodymium iron boron permanent magnet
CN117174420A
Rare earth magnetic alloy sheet, its manufacturing method, sintered rare earth magnetic alloy powder, sintered rare earth magnet, metal powder for bonded magnet, and bonded magnet
CN1526147A
Method for manufacturing r-t-b based sintered magnet