An organic semiconductor modified composite lithium negative electrode and its preparation method and application

By covering the ultra-thin alkylthiophene lithium layer on the surface of the lithium electrode matrix, the problems of dendrite growth and electrolyte reaction of lithium metal negative electrode are solved, uniform deposition of lithium ions and high current density are achieved, and the battery cycle life is extended and the process is simplified. Process, suitable for industrial production.

CN118693233BActive Publication Date: 2024-11-26CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411176252.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

During the battery recycling process, the lithium metal negative electrode has a short life due to irregular growth of dendrites and electrolyte side reactions, and the rapid growth under large currents has caused safety risks, which hinders the expansion and development of lithium metal batteries.

Method used

Using organic semiconductor modified composite lithium negative electrode, the ultra-thin alkylthiophene lithium layer is coated on the surface of the lithium electrode matrix to provide a uniform nucleation area to regulate Li nucleation, achieving uniform deposition of lithium ions and high current density. The preparation method includes mechanical Chemical reactions such as rolling, simplify the process flow.

Benefits of technology

It achieves large capacity and uniform deposition of lithium ions and high current, extends the battery cycle life, reduces the risk of dendrites, simplifies the preparation process and is suitable for industrial production, and the interface potential drops significantly, improving battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118693233B_ABST
    Figure CN118693233B_ABST
Patent Text Reader

Abstract

The present invention provides an organic semiconductor modified composite lithium negative electrode and a preparation method and application thereof, belonging to the technical field of lithium batteries. The interface layer in the composite lithium negative electrode is composited by organic semiconductor molecular units, has a carbon-based skeleton and a sulfur-containing ring, can achieve better lithium affinity behavior and ion diffusion behavior, and can provide active sites for Li nucleation. The sulfur ring on the thiophene unit can be used as a uniform nucleation area to regulate Li nucleation, so that Li atoms are uniformly absorbed and reduced, thereby achieving uniform deposition of lithium ions with large capacity and high current, and realizing reaction molding preparation and processing integrated production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium batteries, and in particular to an organic semiconductor modified composite lithium negative electrode and a preparation method and application thereof. Background Art

[0002] In the past few years, the demand for high energy density battery systems has increased dramatically, and lithium metal has become a strong candidate for the development and application of high energy density batteries with its extremely high theoretical specific capacity (3860mAh / g). Due to some inherent technical difficulties in the application of lithium metal batteries, the specific capacity utilization of lithium-ion battery negative electrode materials under the traditional framework has reached a bottleneck, making it difficult to meet the application requirements of high energy density battery systems.

[0003] The existing patent application CN117080363A discloses an organic-inorganic hybrid layer composite lithium negative electrode and its preparation method and application. The organic-inorganic hybrid layer includes lithium sulfide, lithium phosphate, molybdenum disulfide and organic polyphosphate. Due to the high temperature and high pressure conditions during the friction reaction, the Mo-S bond of the oil film adsorbed on the surface breaks, the oxygen in the lithium metal is replaced by the sulfur in the dithiophosphate, and reacts with the lithium metal to form organic phosphate and inorganic lithium sulfide and lithium phosphate; the middle part is decomposed into inorganic substances such as molybdenum disulfide, and the organic-inorganic hybrid layer is composed of multiple components, which has high electrical conductivity, interface ion diffusion rate and super lithium affinity. However, there is a high cost of the preparation process; CN113540417A discloses a polythiophene-coated single-crystal NCM ternary material, which improves the performance of single-crystal NCM particles by polythiophene coating, and uses polymer conductivity to enhance the conductivity of NCM materials and improve the cyclic stability of the material. However, this method is based on the physical properties of the polymer to achieve performance improvement.

[0004] Currently, lithium metal anodes have a short lifespan due to irregular dendrite growth during battery cycling and adverse side reactions with electrolytes. At the same time, the rapid growth of lithium dendrites under high currents will cause battery volume expansion, increase safety risks, and hinder the further expansion and development of the lithium metal battery market.

[0005] Based on this, the present invention designs an organic semiconductor modified composite lithium negative electrode and a preparation method and application thereof. Summary of the invention

[0006] The present invention provides an organic semiconductor modified composite lithium negative electrode and a preparation method and application thereof, the purpose of which is to solve the above-mentioned problems existing in the background technology.

[0007] In order to achieve the above-mentioned purpose, the embodiments of the present invention provide an organic semiconductor modified composite lithium negative electrode and a preparation method and application thereof. The interface layer in the composite lithium negative electrode is composited by organic semiconductor molecular units, has a carbon-based skeleton and a sulfur-containing ring, can achieve better lithium-philic behavior and ion diffusion behavior, and can provide active sites for the nucleation of Li. The sulfur ring on the thiophene unit can be used as a uniform nucleation area to regulate the nucleation of Li, so that the Li atoms are uniformly absorbed and reduced, thereby realizing uniform deposition of lithium ions with large capacity and high current, and realizing reaction molding preparation and processing integrated production.

[0008] An embodiment of the present invention provides an organic semiconductor modified composite lithium negative electrode, comprising a substrate and an organic semiconductor modified interface layer;

[0009] The matrix contains lithium;

[0010] The organic semiconductor modified interface layer is an ultra-thin alkylthiophene lithium layer having a carbon-based skeleton and a sulfur ring structure; wherein the carbon chain number of the alkyl group is 1 to 14;

[0011] The ultra-thin alkylthiophene lithium layer is 100-5000 nm;

[0012] The symmetric battery assembled with the organic semiconductor modified composite lithium negative electrode has a high conductivity at 1 mA / cm 2 、1 mAh / cm 2 Under the test conditions, a stable cycle of more than 3200 h was achieved.

[0013] According to one aspect of this embodiment, the organic semiconductor modified interface layer is 3-dodecylthiophene lithium.

[0014] According to one aspect of this embodiment, the material of the matrix includes at least one of lithium element, lithium alloy, and lithium-boron composite material.

[0015] Preferably, the lithium alloy chemical formula is Li x M y , M is selected from at least one of sodium, carbon, silicon, magnesium, aluminum, indium, silver, gold, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, germanium, tin, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, cadmium, antimony, hafnium, tantalum, tungsten, rhenium, iridium, platinum, mercury, thallium, lead, bismuth and polonium; x is 0.65-0.95, and y is 0.05-0.35.

[0016] The lithium-boron composite material includes a material whose total mass content of lithium and boron elements is more than 70%. Specifically, by mass percentage, the lithium-boron composite material consists of 65% to 95% Li, 5% to 35% B and 0 to 30% N, wherein the N is selected from at least one of sodium, carbon, silicon, magnesium, aluminum, indium, silver, gold, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, germanium, tin, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, cadmium, antimony, hafnium, tantalum, tungsten, rhenium, iridium, platinum, mercury, thallium, lead, bismuth and polonium.

[0017] The composite material containing at least one of lithium element, lithium alloy and lithium-boron composite material includes but is not limited to a composite material formed by combining at least one of lithium element, lithium alloy or lithium-boron composite material with a porous skeleton or other supporting skeleton by physical or chemical methods; the porous skeleton includes but is not limited to foam copper, foam nickel, copper mesh, nickel mesh, carbon cloth, carbon paper, powder metallurgy porous copper, powder metallurgy porous nickel, porous stainless steel, porous polymer fiber, porous polymer conductive material such as aramid mesh, polyester mesh, acrylic mesh, nylon mesh, polyimide mesh, polypropylene mesh, polytetrafluoroethylene mesh, polyvinylidene fluoride mesh, etc.; the other supporting skeleton includes but is not limited to conductive substrates such as copper, carbon cloth, conductive polymer, etc. Among them, the physical or chemical method includes but is not limited to rolling, stamping, extrusion, vapor deposition and other processes.

[0018] According to one aspect of this embodiment, the thickness of the substrate is 5 μm to 1.5 mm.

[0019] Based on a general concept of the invention, an embodiment of the present invention provides a method for preparing the above-mentioned organic semiconductor modified composite lithium negative electrode, the preparation method comprising: coating alkylthiophene on the surface of a substrate, and obtaining the negative electrode through a mechanochemical reaction.

[0020] According to one aspect of this embodiment, the mechanochemical reaction is selected from at least one of rolling, stamping, and extrusion.

[0021] According to one aspect of this embodiment, during the rolling, stamping or extrusion, the total deformation of the substrate is greater than 0 and less than 100%.

[0022] According to one aspect of this embodiment, the preparation method specifically includes: reacting a 3-dodecylthiophene (P3DDT) solution with zero-valent lithium in a matrix through mechanical rolling.

[0023] According to one aspect of this embodiment, the mass proportion of 3-dodecylthiophene is 1-60%, and the thickening preparation temperature is 10-90°C.

[0024] The embodiments of the present invention also provide the use of the above-mentioned organic semiconductor modified composite lithium negative electrode or the organic semiconductor modified composite lithium negative electrode prepared by the above-mentioned preparation method in an electrochemical energy storage device.

[0025] The electrochemical energy storage device includes but is not limited to lithium-ion batteries, lithium-sulfur batteries, lithium-air batteries, capacitors, etc.

[0026] The above scheme of the present invention has the following beneficial effects:

[0027] (1) The present invention protects the lithium-containing substrate by coating the surface of the electrode substrate with a thiophene-based lithium layer as an interface protection layer, thereby inducing uniform deposition of lithium ions and maintaining dynamic stability on the negative electrode surface; at the same time, it prevents the electrolyte from reacting with the lithium-containing electrode, stabilizes the electrode interface, and has high lithium ion conductivity and strong lithium affinity.

[0028] (2) The organic semiconductor modified composite lithium negative electrode of the present invention is applied to lithium batteries, which can realize high current density and high rate application of lithium negative electrode, and effectively solve the problem of dendrite growth of lithium negative electrode under such conditions.

[0029] (3) The preparation method of the present invention has a simple process and a convenient flow, and can be used in industrial production. In addition, the organic semiconductor modified interface layer has an ultra-low interface potential. Compared with the untreated substrate, the interface potential of the composite electrode material is reduced by 3 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 is an optical image of the electrode material surface of Example 1 and Comparative Example 1 of the present invention; wherein, Figure 1 a is the optical image of the electrode material surface of Comparative Example 1, Figure 1 b is an optical image of the electrode material surface of Example 1;

[0032] Figure 2 is an XPS graph of the composite lithium negative electrode of Example 1 of the present invention; wherein, Figure 2 a is the XPS peak simulation analysis of C 1s of the composite lithium anode (Li@P3DDT). Figure 2 b is the XPS peak simulation analysis of O 1s of the composite lithium anode (Li@P3DDT). Figure 2 c is the XPS peak simulation analysis of S 2p of the composite lithium anode (Li@P3DDT). Figure 2 d is the XPS peak simulation analysis of Li 1s of the composite lithium anode (Li@P3DDT);

[0033] Figure 3 is the XPS graph of the lithium metal pole piece material in Comparative Example 1 of the present invention; wherein, Figure 3 a is the XPS peak simulation analysis of C 1s of lithium metal electrode. Figure 3 b is the XPS peak simulation analysis of O 1s of lithium metal electrode. Figure 3 c is the XPS peak simulation analysis of Li 1s of lithium metal electrode;

[0034] Figure 4 It is a microscopic morphology of the electrode of lithium deposition in Comparative Example 1 and Example 1 of the present invention; wherein, Figure 4 a and Figure 4 c are the microscopic morphology images of the 100μm and 10μm lithium-deposited electrodes of Comparative Example 1, Figure 4 b and Figure 4 d are microscopic morphology images of the electrode with 100 μm and 10 μm lithium deposition in Example 1 respectively;

[0035] Figure 5 It is a microscopic morphology of the pole piece de-lithiated in Comparative Example 1 and Example 1 of the present invention; wherein, Figure 5 a and Figure 5 c are microscopic morphology pictures of 20μm and 5μm lithium-free pole pieces of comparative example 1, Figure 5 b and Figure 5 d are microscopic morphology images of 20 μm and 5 μm de-lithiated electrodes of Example 1;

[0036] Figure 6 It is the microscopic morphology of the pole piece after the cycle of comparative example 1 and embodiment 1 of the present invention; wherein, Figure 6 a and Figure 6 c are the microscopic morphology of the electrode after 20μm and 5μm cycles of comparative example 1, Figure 6 b and Figure 6 d are the microscopic morphology images of the electrode after 20 μm and 5 μm cycles of Example 1;

[0037] Figure 7 is a comparison diagram of the elastic modulus of the pole pieces of Comparative Example 1 and Example 1 of the present invention;

[0038] Figure 8 is a comparison chart of the hardness of the pole pieces of Comparative Example 1 and Example 1 of the present invention;

[0039] Fig. 9 is the interfacial electrostatic potential of the electrode materials prepared in Example 1 and Comparative Example 1 of the present invention measured in the KPFM mode under an atomic force microscope; wherein, Fig. 9 a is the interfacial electrostatic potential of the electrode material prepared in Example 1 measured in the KPFM mode under an atomic force microscope, Fig. 9 b is the interfacial electrostatic potential of the electrode material prepared in Comparative Example 1 measured in the KPFM mode under an atomic force microscope;

[0040] Fig.10 The electrode materials of Example 1, Comparative Example 1 and Comparative Example 3 of the present invention are respectively 2 、1mAh / cm 2 Cycling performance diagram of symmetrical battery under test conditions;

[0041] Fig.11 The electrode materials of Example 1 and Comparative Example 1 of the present invention are respectively 2 、5mAh / cm 2 Cycling performance diagram of symmetrical battery under test conditions;

[0042] Fig.12 The cycle efficiency diagram of the full battery assembled with lithium cobalt oxide and the electrode materials of Example 1 and Comparative Example 1 of the present invention at a rate of 1C, with a positive electrode active material loading of 12 mg cm -2 ;

[0043] Fig.13 The electrode materials of Example 2 and Comparative Example 2 of the present invention are respectively 2 、1 mAh / cm 2 Cycling performance diagram of a symmetric battery under test conditions. DETAILED DESCRIPTION

[0044] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0045] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0046] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0047] "Lithium deposition" refers to the microscopic morphology formed by the deposition of lithium ions on the surface of the electrode after battery cycling.

[0048] "Delithiation" refers to the microscopic morphology formed on the surface of the electrode sheet after the battery is cycled and lithium ions are delithiated.

[0049] In view of the above-mentioned problems existing in the background technology, the present invention provides an organic semiconductor modified composite lithium negative electrode and its preparation method and application. The present invention can induce uniform deposition of lithium ions and keep the negative electrode surface dynamically stable by coating an ultra-thin thiophene-based lithium layer on the surface of the electrode substrate as an interface protection layer to protect the lithium-containing substrate; at the same time, it prevents the electrolyte from reacting with the lithium-containing electrode, stabilizes the electrode interface, and has high lithium ion conductivity and strong lithium affinity. The organic semiconductor modified composite lithium negative electrode is applied to lithium batteries, which can realize the high current density and high rate application of lithium negative electrodes, and effectively solve the problem of dendrite growth of lithium negative electrodes under such conditions. It has a preparation method, a simple process, and a simple flow, and can be matched with industrial production. In addition, the organic semiconductor modified interface layer has an ultra-low interface potential. Compared with the untreated substrate, the interface potential of the composite electrode material is reduced by 3 times.

[0050] The following will describe in detail with reference to specific embodiments.

[0051] Example 1

[0052] This embodiment provides a method for preparing an organic semiconductor modified composite lithium negative electrode.

[0053] The preparation method of this embodiment comprises the following steps:

[0054] The prepared 3-dodecylthiophene solution (3-dodecylthiophene mass fraction of 5%) was coated on the surface of the lithium metal sheet, and the 3-dodecylthiophene was 205wt% of the mass of the metal lithium sheet (substrate thickness of 150 microns); the composite lithium negative electrode was obtained by room temperature rolling with a reduction of 16.67%, and the pole piece with a diameter of 16 mm (thickness of 100 microns) was punched out.

[0055] After testing, the optical photos of its surface are as follows Figure 1 b; the surface composition is as follows Figure 2 The surface electrostatic potential was tested and the results are shown in Fig. 9 As shown in a, it can be seen that the surface electrostatic potential decreases by 3 times.

[0056] In the glove box, the above-mentioned electrode and lithium sheet were assembled into button cells, Celgard2400 was used as the separator, the electrolyte was 1M LiTFSI DME:DOL=1:1 (volume ratio), containing 2% LiNO3 additive, and constant current charge and discharge tests were carried out at 1 mA / cm 2 、1 mAh / cm 2 Symmetrical battery cycle test was carried out under test conditions, and the test results are as follows Fig.10 As shown in Figure 2, it can achieve stable cycling for more than 1600 cycles (3200 hours) with the polarization voltage still not exceeding 0.2V; at 5 mA / cm 2 、5 mAh / cm2 Symmetrical battery cycle test was carried out under test conditions, and the test results are as follows Fig.11 As shown in the figure, under high current and high capacity, the battery can be stably cycled for more than 600 cycles (650 hours); the polarization voltage still does not exceed 0.5V; the surface morphology after cycling is as follows Figure 6 b and Figure 6 As shown in d.

[0057] The full battery was assembled with a composite electrode with a diameter of 16 mm and a LiCoO2 positive electrode, Celgard2400 was used as a separator, and the electrolyte was 1.0M LiPF6 EC:EMC:FEC=1:1:1 (volume ratio). The full battery cycle test was carried out under 1C test conditions. Fig.12 As shown, the capacity retention rate after 180 cycles can reach 99.9%.

[0058] Comparative Example 1

[0059] The surface of the original commercial lithium strip is as follows Figure 1 As shown in a. Two commercial lithium ribbons (Zhongneng Lithium) were used as positive and negative electrodes to assemble button-type symmetrical cells, Celgard2400 was used as the separator, and the electrolyte was 1M LiTFSI DME:DOL=1:1 (volume ratio), containing 2% LiNO3 additive. Symmetrical battery cycle test was carried out under the same test conditions as in Example 1, 1 mA / cm 2 、1 mAh / cm 2 Test results such as Fig.10 , it can only stably cycle 30 times, and the polarization voltage surges to 0.5V; 5 mA / cm 2 、5 mAh / cm 2 Test results such as Fig.11 , it can only stably cycle 50 times, and the polarization voltage surges to 0.4V.

[0060] A full battery was assembled using commercial lithium ribbon as the negative electrode and LiCoO2 as the positive electrode, Celgard2400 was used as the separator, and the electrolyte was 1.0M LiPF6 EC:EMC:FEC=1:1:1 (volume ratio). A full battery cycle test was carried out under the same test conditions as in Example 1. The test results are shown in Figure 2. Fig.12 As shown in Figure 1, at a rate of 1C, the capacity decays to 25.8% after 180 cycles. As the rate increases, the discharge specific capacity is always lower than that of Example 1.

[0061] Example 2

[0062] This embodiment provides a method for preparing an organic semiconductor modified composite lithium negative electrode.

[0063] The preparation method of this embodiment comprises the following steps:

[0064] The prepared 3-dodecylthiophene solution (3-dodecylthiophene mass fraction of 5%) was coated on the surface of lithium-boron metal sheet (mass fraction 90% Li 10% B); the room temperature rolling method was used with a reduction of 16.67% to obtain a composite negative electrode based on lithium-boron metal, and the pole piece with a diameter of 16 mm (thickness of 100 microns) was punched out.

[0065] In the glove box, the pole piece and the lithium boron sheet were assembled into a button cell, Celgard2400 was used as the separator, the electrolyte was 1M LiTFSI DME:DOL=1:1 (volume ratio), containing 2% LiNO3 additive, and the pole piece was subjected to constant current charge and discharge test at 1mA / cm 2 、1 mAh / cm 2 Symmetrical battery cycle test was carried out under test conditions, and the test results are as follows Fig.13 As shown, it is possible to achieve stable cycling for more than 300 cycles (600 hours); the polarization voltage still does not exceed 0.2V.

[0066] Comparative Example 2

[0067] Two commercial lithium-boron strips were used as positive and negative electrodes to assemble button-type symmetrical cells, Celgard 2400 was used as the separator, and the electrolyte was 1M LiTFSI DME:DOL = 1:1 (volume ratio), containing 2% LiNO3 additive. Symmetrical cell cycle test was carried out under the same test conditions as in Example 2, 1 mA / cm 2 、1 mAh / cm 2 Test results such as Fig.13 , it can only stably cycle 30 times (about 60 hours), and the polarization voltage surges to 0.5V.

[0068] Comparative Example 3

[0069] The prepared 3-propylthiophene solution (3-propylthiophene solution mass fraction of 5%) was coated on the surface of the lithium metal sheet, and the composite lithium negative electrode was obtained by room temperature rolling with a reduction of 16.67%, and the pole piece with a diameter of 16 mm (thickness of 100 microns) was punched out.

[0070] In a glove box, the above-mentioned pole piece and lithium sheet were assembled into button cells, Celgard2400 was used as a separator, the electrolyte was 1M LiTFSI DME:DOL=1:1 (volume ratio), containing 2% LiNO3 additive, and constant current charge and discharge test was carried out. A symmetrical battery cycle test was carried out under the same test conditions as in Example 1, 1 mA / cm 2 、1 mAh / cm 2 Test results such as Fig.10As shown, it can only stably cycle for 380 cycles (about 760 hours), and the polarization voltage surges to about 0.3V.

[0071] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An organic semiconductor modified composite lithium negative electrode, characterized in that: including a substrate and an organic semiconductor modified interface layer; The matrix contains lithium; The organic semiconductor modified interface layer is an ultra-thin alkylthiophene lithium layer having a carbon-based skeleton and a sulfur ring structure; wherein the carbon chain number of the alkyl group is 1 to 14; The ultra-thin alkylthiophene lithium layer is 100-5000 nm; The symmetric battery assembled with the organic semiconductor modified composite lithium negative electrode has a high conductivity at 1 mA / cm 2 and 1 mAh / cm 2 Under the test conditions, a stable cycle of more than 3200 h was achieved.

2. The organic semiconductor modified composite lithium negative electrode according to claim 1, characterized in that: The organic semiconductor modified interface layer is 3-dodecylthiophene lithium.

3. The organic semiconductor modified composite lithium negative electrode according to claim 1, characterized in that: The material of the matrix includes at least one of lithium element, lithium alloy and lithium-boron composite material.

4. The organic semiconductor modified composite lithium negative electrode according to claim 1, characterized in that: The thickness of the substrate is 5 μm to 1.5 mm.

5. A method for preparing an organic semiconductor modified composite lithium negative electrode as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises: coating alkylthiophene on the surface of a substrate and performing a mechanochemical reaction to obtain the alkylthiophene.

6. The method for preparing an organic semiconductor modified composite lithium negative electrode according to claim 5, characterized in that: The mechanochemical reaction is selected from at least one of rolling, stamping and extrusion.

7. The method for preparing an organic semiconductor modified composite lithium negative electrode according to claim 6, characterized in that: During the rolling, stamping or extrusion, the total deformation of the substrate is greater than 0 and less than 100%.

8. The method for preparing an organic semiconductor modified composite lithium negative electrode according to claim 5, characterized in that: The preparation method specifically comprises: reacting a 3-dodecylthiophene solution with zero-valent lithium in a matrix through mechanical rolling to obtain the product.

9. The method for preparing an organic semiconductor modified composite lithium negative electrode according to claim 8, characterized in that: The mass proportion of 3-dodecylthiophene in the 3-dodecylthiophene solution is 1-60%, and the thickening preparation temperature is 10-90°C.

10. Use of an organic semiconductor-modified composite lithium negative electrode as claimed in any one of claims 1 to 4 or an organic semiconductor-modified composite lithium negative electrode prepared by the preparation method as claimed in any one of claims 5 to 9 in an electrochemical energy storage device.