Preparation of heteroatom-doped amorphous carbon-coated silicon-carbon composite materials by silane cracking method and its application
By doping metal and nanosilicon in porous carbon and depositing heteroatoms doping amorphous carbon on the outer layer to form a silicon-carbon composite material with core-shell structures, the shortcomings of the new silicon-carbon materials in high-temperature storage and rate performance are solved. It significantly improves the electronic conductivity and rate performance, improves the circulation performance and liquid absorption and liquid retention ability.
Patent Information
- Application Number
- CN202411163034.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The new silicon carbon materials have shortcomings in high-temperature storage and rate performance, mainly due to the poor electronic conductivity of porous carbon and the defects in core structure, resulting in material performance deviations.
Heteroatom doped amorphous carbon is used to coat the silicon-carbon metal composite material, and the electron conductivity and rate performance of the material are improved by doping metal and nanosilicon in porous carbon and depositing heteroatom doping amorphous carbon on the outer layer. Specific steps include the preparation of metal-doped porous carbon and silane cleavage and deposition on the basis of it to form a core-shell structure.
It significantly improves the electronic conductivity and rate performance of the material, improves the first-time efficiency and circulation performance, reduces gas production, and enhances high-temperature storage capacity and liquid absorption and liquid retention capacity.
Smart Images

Figure CN118693266B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium ion battery material preparation, and specifically provides a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material, and a silane cracking method preparation method and application thereof. Background Art
[0002] Compared with the traditional silicon carbon prepared by sand milling, the new silicon carbon material prepared by silane cracking method is used in the fields of high energy density lithium ion batteries due to its high specific capacity, low expansion, good cycle performance and other characteristics. However, since the raw materials for preparing the new silicon carbon material are composed of porous carbon and its silane, and the porous carbon itself has poor electronic conductivity and many porous structural defects in the inner core, the rate performance deviation of the material and its high temperature storage are slightly poor. In this field, one of the measures to improve the high temperature storage and rate of the material is to dope and coat the inner core and outer shell of the porous carbon. Metals and their compounds are often used as doping and coating materials to form new silicon carbon materials because of their advantages such as high electronic conductivity, so as to reduce the surface defects of the material, improve the electronic conductivity of the material, and improve the rate performance. Summary of the invention
[0003] In order to improve the rate performance and first efficiency of the new silicon-carbon material, the present invention provides a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material, and a preparation method and application thereof by a silane cracking method.
[0004] The first aspect of the present invention provides a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material, which presents a core-shell structure, with nano-silicon and metal-doped porous carbon as the core and heteroatom-doped amorphous carbon as the shell; calculated based on the mass ratio of the composite material as 100%, the mass ratio of the shell is 3-10wt%, preferably 5-10wt%.
[0005] A second aspect of the present invention provides a method for preparing a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material by a silane cracking method, comprising the following steps:
[0006] (1) The preparation method of metal-doped porous carbon is as follows: 100 parts by mass of phenolic resin, 1-5 parts by mass of metal nitrate compound, and 1-5 parts by mass of inorganic lithium salt are added to 500-1000 parts by mass of acetone and dispersed evenly, spray dried, and introduced with carbon dioxide at a temperature of 200-300°C for pre-oxidation treatment for 1-6 hours, and then placed in a tubular furnace and heated to 800-1200°C in an inert atmosphere for carbonization treatment for 1-6 hours, and then cooled to room temperature in an argon atmosphere to obtain metal-doped porous carbon.
[0007] (2) The metal-doped porous carbon prepared above is transferred to a tubular furnace, and a mixed gas of silane and metal hydride is introduced at the same time at a pressure of 1-2 MPa and a temperature of 400-600°C to deposit nano-silicon and metal in the porous carbon. The temperature is then raised to 700-1000°C, and a mixed gas of a heteroatom carbon source is introduced for vapor phase deposition to obtain a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material.
[0008] Wherein, the metal nitrate compound is selected from one or more of iron nitrate, silver nitrate, copper nitrate and nickel nitrate; the inorganic lithium salt is selected from one or more of lithium carbonate, lithium hydroxide, lithium titanate and lithium cobaltate.
[0009] Wherein, the metal hydride is selected from one or more of magnesium dihydride, lithium hydride, sodium hydride and copper hydride.
[0010] Wherein, the flow rate of the silane is 100-500 SCCM, and the ventilation time is 60-600 min; the flow rate of the metal hydride is 10-50 SCCM, and the ventilation time is 60-600 min.
[0011] The heteroatom mixed gas is composed of one of ammonia, phosphine, and sulfur dioxide mixed with one of methane, ethane, acetylene, and ethylene, with a mixing volume ratio of 1-5:10, a flow rate of 10-100 SCCM, and a ventilation time of 1-6 hours.
[0012] A third aspect of the present invention provides a negative electrode plate for a lithium ion battery, comprising a negative electrode current collector and a negative electrode material coated on at least one surface of the negative electrode current collector, wherein the negative electrode material comprises the above-mentioned silicon-carbon composite material.
[0013] A fourth aspect of the present invention provides a lithium ion battery comprising the above-mentioned negative electrode plate, which also includes a positive electrode plate and a separator between the positive electrode plate and the negative electrode plate.
[0014] Beneficial effects of the present invention
[0015] (1) By doping metals into porous carbon, the electronic conductivity of the material is improved, while doping lithium salt compounds is used to improve the initial efficiency of the material.
[0016] (2) By decomposing silane in metal-doped porous carbon to deposit nanosilicon and decomposing metal hydrides to generate metal, the electronic conductivity of the material is improved, thereby improving the rate performance.
[0017] (3) Materials Carbon dioxide is used to form pores in the silicon-carbon precursor and then oxidize it to produce metal-doped porous carbon, which improves the electronic conductivity of the material.
[0018] (4) By coating the outer layer with heteroatom-doped amorphous carbon, the inner core silicon is prevented from directly contacting the electrolyte, thereby reducing gas production and improving the initial efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to make the purpose, technical solution and beneficial effects of the present invention clearer, the present invention provides the following drawings for illustration:
[0020] Figure 1 This is a SEM image of the heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material prepared in Example 1. DETAILED DESCRIPTION
[0021] The heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material and its application provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0022] Example 1
[0023] A method for preparing a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material:
[0024] The preparation method of metal-doped porous carbon is as follows: 100g of phenolic resin, 3g of silver nitrate, and 3g of lithium carbonate are added to 1000g of acetone and dispersed evenly, and then the resulting material is transferred to a tubular furnace by spray drying, and pre-oxidized for 3 hours at a temperature of 250°C by passing carbon dioxide gas, and then placed in a tubular furnace and heated to 900°C under an argon inert atmosphere for carbonization treatment for 3 hours, and then cooled to room temperature under an argon atmosphere to obtain metal-doped porous carbon.
[0025] The metal-doped porous carbon was transferred to a tubular furnace, and at a pressure of 1.5 MPa and a temperature of 500°C, a mixed gas of silane gas (flow rate 300 SCCM, time 300 min) and magnesium dihydride (flow rate 30 SCCM, time 300 min) was introduced simultaneously to deposit nano-silicon and metallic magnesium in the porous carbon. The temperature was then raised to 900°C, and an ammonia / methane mixed gas (volume ratio, ammonia: methane = 3:10, flow rate 50 SCCM) was introduced for vapor deposition for 3 hours to obtain a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material.
[0026] Example 2
[0027] A method for preparing a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material:
[0028] The preparation method of metal-doped porous carbon is as follows: 100g of phenolic resin, 1g of ferric nitrate, and 1g of lithium hydroxide are added to 1000g of acetone and dispersed evenly, and then the obtained material is transferred to a tubular furnace by spray drying, and carbon dioxide is introduced at a temperature of 200°C for pre-oxidation treatment for 6 hours, and then placed in a tubular furnace and heated to 800°C under an argon inert atmosphere for carbonization treatment for 6 hours, and then cooled to room temperature under an argon atmosphere to obtain metal-doped porous carbon.
[0029] The metal-doped porous carbon was transferred to a tubular furnace, and a mixed gas of silane gas (flow rate 100 SCCM, time 600 min) and lithium hydride (flow rate 10 SCCM, time 600 min) was introduced simultaneously at a pressure of 1 MPa and a temperature of 600°C to deposit nano-silicon and metal in the porous carbon. The temperature was then raised to 700°C, and a phosphine / acetylene mixed gas (volume ratio, phosphine: acetylene = 1:10, flow rate 10 SCCM) was introduced for vapor deposition for 6 hours to obtain a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material.
[0030] Example 3
[0031] A method for preparing heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material by silane cracking method:
[0032] The preparation method of metal-doped porous carbon is as follows: 100g of phenolic resin, 5g of copper nitrate, and 5g of lithium titanate are added to 1000g of acetone and dispersed evenly, then spray-dried, and then pre-oxidized for 6 hours at a temperature of 300°C by introducing carbon dioxide, and then placed in a tubular furnace and heated to 1200°C under an argon inert atmosphere for carbonization treatment for 1 hour, and then cooled to room temperature under an argon atmosphere to obtain metal-doped porous carbon.
[0033] The metal-doped porous carbon was transferred to a tubular furnace, and a mixed gas of silane gas (gas flow rate 500 SCCM, time 60 min) and sodium hydride (gas flow rate 50 SCCM, time 60 min) was introduced simultaneously at a pressure of 2 MPa and a temperature of 400°C to deposit nanosilicon and metallic sodium in the porous carbon. The temperature was then raised to 1000°C, and a sulfur dioxide / ethylene mixed gas (volume ratio, sulfur dioxide: ethylene = 5:10, flow rate 100 SCCM) was introduced for vapor deposition for 1 hour to obtain a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material.
[0034] Comparative Example 1:
[0035] The difference from Example 1 is that porous carbon is used to replace metal-doped porous carbon, and the rest is the same as Example 1.
[0036] Comparative Example 2:
[0037] The difference from Example 1 is that only silane gas is introduced, and magnesium hydride gas is not introduced.
[0038] Comparative Example 3:
[0039] The difference from Example 1 is that the heteroatom carbon source mixed gas (ammonia:methane volume ratio 3:10) is replaced by methane gas.
[0040] Test Case
[0041] 1. SEM test:
[0042] Figure 1 This is a SEM image of the heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material prepared in Example 1. It can be seen from the figure that the material has a granular structure with a particle size between 5-10µm, and the rough small particles on the surface of the material are deposited heteroatom-doped amorphous carbon.
[0043] 2. Physical and chemical tests and button battery tests:
[0044] According to the method in the national standard GB / T 38823-2020 "Silicon Carbon", the specific surface area, tap density, and carbon content of each silicon-carbon composite material obtained in Examples 1-3 and Comparative Examples 1-3 were respectively measured, and the electrical conductivity of each silicon-carbon composite material was tested using a four-probe tester; the test results are shown in Table 1 below.
[0045] The silicon-carbon composite materials obtained in Examples 1-3 and Comparative Examples 1-3 were used as active materials for the negative electrode plates of the battery and were respectively prepared and assembled into 8 button batteries; wherein the specific preparation process of each button battery is as follows:
[0046] Preparation of battery negative electrode sheets: Add a binder, a conductive agent and a solvent to each silicon-carbon composite material (as the active material of the battery negative electrode sheet) corresponding to Examples 1-3 and Comparative Examples 1-3, stir to make a slurry, apply it on a copper foil, dry and roll to obtain each battery negative electrode sheet; wherein the binder is LA132 binder, the conductive agent is SP (conductive carbon black), and the solvent is NMP, and the ratio is: silicon-carbon composite material: SP: LA132: NMP = 95g: 1g: 4g: 220mL;
[0047] Preparation of button cells: LiPF6 solution was used as the electrolyte, wherein the concentration of LiPF6 was 1 mol / L, and the solvent used was a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DMC) in a weight ratio of 1:1; a metal lithium sheet was used as the counter electrode, and a polypropylene (PP) film was used as the diaphragm. The simulated battery was assembled in an argon-filled glove box, and the electrochemical performance was performed on a Wuhan Blue Electric CT2001A battery tester. The test conditions were: the charge and discharge voltage range was 0.005V to 2.0V, and the charge and discharge rate was 0.1C; a full-charge expansion test was also performed: the thickness D1 of the negative electrode sheet of the button cell after rolling was tested, and then the negative electrode sheet of the button cell was dissected when it was fully charged to 100% SOC, and the thickness D2 of the negative electrode sheet was tested, and then the full-charge expansion rate = (D2-D1) / D1*100% was calculated; the test results are shown in Table 1 below.
[0048] Table 1
[0049] First discharge specific capacity (mAh / g) First efficiency (%) Carbon content <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Tap density (g / cm 3 )]]> Powder conductivity (S / cm) Fully charged expansion Silicon grain(nm) Example 1 1838.6 91.7 48.2% 5.9 1.02 1.23 59.9% 1.5 Example 2 1881.7 91.9 47.9% 7.1 1.05 2.17 64.3% 1.9 Example 3 1811.4 90.9 48.6% 6.3 0.97 0.89 57.8% 1.4 Comparative Example 1 1764.5 88.3 49.9% 4.5 0.90 0.23 82.0% 2.3 Comparative Example 2 1812.5 87.5 50.6% 4.2 0.88 0.45 77.3% 2.1 Comparative Example 3 1822.4 89.1 49.5% 4.9 0.93 0.78 67.3% 2.0
[0050] It can be seen from Table 1 above that the button cells made of the silicon-carbon composite materials provided in Examples 1-3 of the present application are significantly better than those in Comparative Examples 1-3 in terms of first discharge specific capacity and first efficiency; the reason may be that the material of the present application uses metal-doped porous carbon to improve the electronic conductivity of the material, reduce the polarization of the material, and improve the specific capacity of the material; at the same time, the material is doped with lithium salt compounds to improve the first efficiency of the material.
[0051] 3. Soft pack battery test:
[0052] The silicon-carbon composite materials obtained in Examples 1-3 and Comparative Examples 1-3 were doped with 90% artificial graphite as negative electrode materials (i.e., negative electrode plates), and the ternary material LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 is used as the positive electrode material, the electrolyte and the diaphragm to assemble a 5Ah soft-pack battery; the diaphragm of the soft-pack battery is Celegard 2400, the electrolyte is LiPF6 solution, the solvent of the LiPF6 solution is a mixed solution of EC and DEC with a volume ratio of 1:1, and the concentration of LiPF6 is 1.3mol / L; the following performance tests are carried out on each soft-pack battery:
[0053] A. Liquid absorption capacity test: Use a 1mL burette and absorb 1mL of electrolyte, add a drop of electrolyte on the surface of the negative electrode, and time it until the electrolyte is completely absorbed, and record the time t; the test results are shown in Table 2.
[0054] B. Liquid retention rate test: Calculate the theoretical liquid absorption of the negative electrode m1 according to the electrode parameters, and weigh the weight of the negative electrode m2. Then, soak the negative electrode in the electrolyte for 24 hours, weigh the weight of the negative electrode m3, calculate the liquid absorption of the negative electrode m3-m2, and calculate according to the following formula: Liquid retention rate = (m3-m2)*100% / m1; the test results are shown in Table 2 below.
[0055] Table 2
[0056] Liquid suction speed (S) Fluid retention rate Example 1 34 91.4% Example 2 26 90.1% Example 3 42 89.9% Comparative Example 1 76 85.9% Comparative Example 2 89 84.7% Comparative Example 3 82 84.1%
[0057] It can be seen from Table 2 above that the liquid absorption and liquid retention capabilities of the silicon-carbon composite materials provided in Examples 1-3 of the present application are significantly higher than those of Comparative Examples 1-3. The reason is that the materials in Examples 1-3 have a high specific surface area, which improves the liquid absorption and liquid retention capabilities of the materials.
[0058] C. Rate and cycle performance: Perform cycle performance test and rate test on each soft pack battery;
[0059] Among them, the test conditions of the cycle performance test are: charge and discharge voltage range of 2.5~4.2V, temperature of 25±3.0℃, charge and discharge rate of 1.0C / 1.0C, and cycle number of 500 times; see Table 3 for details; the test conditions of the rate test are: testing the capacity retention rate under the charging rate (0.2C / 0.5C / 1C / 2C / 3C); the test results are shown in Table 4 below.
[0060] Table 3
[0061] Silicon Carbon Composite Materials Initial capacity retention rate (%) Capacity retention after 500 cycles (%) Example 1 100 93.1 Example 2 100 92.2 Example 3 100 91.8 Example 1 100 85.5 Comparative Example 2 100 84.9 Comparative Example 3 100 86.6
[0062] It can be seen from Table 3 that the cycle performance of the example material is significantly better than that of the comparative example. The reason is that the example material has low expansion and small silicon reduction, which reduces the expansion of the battery during its cycle and improves the cycle performance.
[0063] Table 4
[0064] Silicon Carbon Composite Materials 0.2C 0.5C 1C 2C 3C Example 1 100% 98.6% 97.4% 95.6% 91.8% Example 2 100% 99.2% 97.9% 95.9% 92.2% Example 3 100% 98.1% 97.0% 95.1% 91.1% Comparative Example 1 100% 95.4% 94.2% 92.4% 88.3% Comparative Example 2 100% 96.1% 94.8% 92.7% 88.9% Comparative Example 3 100% 96.9% 95.2% 93.1% 89.3%
[0065] It can be seen from Table 4 above that the soft-pack lithium-ion batteries prepared using the silicon-carbon composite materials provided in Examples 1-3 of the present application have better rate performance than those of Comparative Examples 1-3. The main reason for this may be that the silicon-carbon composite materials provided in the examples of the present application have high powder conductivity and large specific surface area, which improves the rate performance of the material.
[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that several improvements and modifications may be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention and do not deviate from the scope defined by the claims of the present invention.
Claims
1. A heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material, characterized in that: The composite material presents a core-shell structure, with nano-silicon and metal-doped porous carbon as the core and heteroatom-doped amorphous carbon as the shell; based on the composite material mass ratio of 100%, the mass ratio of the shell is 3-10wt%; The composite material is obtained according to the following preparation method, which comprises the following steps: (1) adding phenolic resin, metal nitrate compound, inorganic lithium salt or lithium hydroxide to acetone and dispersing them uniformly, spray drying, introducing carbon dioxide at a temperature of 200-300°C for pre-oxidation treatment for 1-6 hours, then placing in a tube furnace, and heating to 800-1200°C in an inert atmosphere for carbonization treatment for 1-6 hours, and then cooling to room temperature in an argon atmosphere to obtain metal-doped porous carbon; (2) transferring the metal-doped porous carbon to a tube furnace, and introducing silane gas and metal hydride mixed gas at the same time at a pressure of 1-2 Mpa and a temperature of 400-600°C to deposit nano-silicon and metal in the porous carbon material, and then heating to 700-1000°C, introducing a heteroatom carbon source mixed gas for vapor phase deposition to obtain a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material; The metal nitrate compound is selected from one or more of iron nitrate, silver nitrate, copper nitrate, and nickel nitrate; the heteroatom mixed gas is a mixture of one of ammonia, phosphine, and sulfur dioxide and one of methane, ethane, acetylene, and ethylene, and the mixing volume ratio is 1-5:10; the inorganic lithium salt is selected from one or more of lithium carbonate, lithium titanate, and lithium cobaltate.
2. The method for preparing the heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material according to claim 1, characterized in that: The method comprises the following steps: (1) adding phenolic resin, metal nitrate compound, inorganic lithium salt or lithium hydroxide to acetone and dispersing the mixture uniformly, spray drying the mixture, introducing carbon dioxide at a temperature of 200-300°C for pre-oxidation treatment for 1-6 hours, placing the mixture in a tube furnace, heating the mixture to 800-1200°C in an inert atmosphere for carbonization treatment for 1-6 hours, and then cooling the mixture to room temperature in an argon atmosphere to obtain metal-doped porous carbon; (2) transferring the metal-doped porous carbon to a tube furnace, and introducing silane gas and a metal hydride mixed gas at a pressure of 1-2Mpa and a temperature of 400-600°C to deposit nano-silicon and metal in the porous carbon material, and then heating the mixture to 700-1000°C, introducing a heteroatom carbon source mixed gas for vapor phase deposition to obtain a heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material; The metal nitrate compound is selected from one or more of iron nitrate, silver nitrate, copper nitrate, and nickel nitrate; the heteroatom mixed gas is a mixture of one of ammonia, phosphine, and sulfur dioxide and one of methane, ethane, acetylene, and ethylene, and the mixing volume ratio is 1-5:10; the inorganic lithium salt is selected from one or more of lithium carbonate, lithium titanate, and lithium cobaltate.
3. The preparation method according to claim 2, characterized in that: The mass ratio of the phenolic resin, the metal nitrate compound, the inorganic lithium salt and the acetone is 100:1-5:1-5:500-1000.
4. The preparation method according to claim 2, characterized in that: The metal hydride is selected from one or more of magnesium dihydride, lithium hydride, sodium hydride and copper hydride.
5. The preparation method according to claim 2, characterized in that: The flow rate of the silane is 100-500 SCCM, and the ventilation time is 60-600 min; the flow rate of the metal hydride is 10-50 SCCM, and the ventilation time is 60-600 min.
6. The preparation method according to claim 2, characterized in that: The ventilation time of the heteroatom mixed gas is 1-6h.
7. A negative electrode plate for a lithium ion battery, characterized in that: The negative electrode plate includes a negative electrode current collector and a negative electrode material coated on at least one surface of the negative electrode current collector, and the negative electrode material includes the heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material according to claim 1 or the heteroatom-doped amorphous carbon-coated silicon-carbon metal composite material prepared by the preparation method according to any one of claims 2-6.
8. A lithium ion battery, characterized in that: The lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet and a separator separated between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet is the negative electrode sheet of the lithium-ion battery according to claim 7.
Citation Information
Patent Citations
Low-expansion long-life silicon-carbon composite material and preparation method thereof
CN115911326A
Metal-doped silicon-carbon composite material as well as preparation method and application thereof
CN116779835A
Cited By
A high-power petroleum coke-based silicon-carbon material and a method for preparing the same
CN122940172A