Anode catalyst layer for fuel cell and preparation method and application thereof

By using multi-stage treatment technology of materials such as platinum carbon catalysts and photoinitiators in hydrogen fuel cells, a catalyst layer with multi-dimensional pores is formed, which solves the problem of low reaction rate of the positive electrode catalyst and significantly improves the diffusion ability and catalytic efficiency of the catalyst layer. .

CN118693296BActive Publication Date: 2024-11-08THINKRE MEMBRANE MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160721.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The reaction rate of the positive electrode catalyst in hydrogen fuel cells is lower than that of the negative electrode, resulting in limited overall reaction rate and uneven catalyst distribution, which faces challenges in improving the proton, electron, and oxygen transfer efficiency and catalytic efficiency of the catalyst layer.

Method used

A mixture of platinum carbon catalyst, ionomer, composite solvent, photoinitiator and α-alkenyl sulfonic acid is coated on the proton exchange membrane after grinding and mixing, and is irradiated with ultraviolet light and staged heat treatment to form a multi-dimensional pore. The catalyst layer improves the diffusion ability of the catalyst layer.

Benefits of technology

The diffusion capacity of protons, reaction gas and water of the catalyst layer is significantly improved, the catalytic efficiency is improved, the oxygen permeability and proton conductivity of the catalyst layer are enhanced, and the mechanical strength and interlayer peeling strength of the catalyst layer and the proton exchange membrane are improved. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GVGU1CPNGCRNU1IO7NB27BJPLEEOZM7DCFYRMWLU
    Figure GVGU1CPNGCRNU1IO7NB27BJPLEEOZM7DCFYRMWLU
Patent Text Reader

Abstract

The present invention discloses an anode catalyst layer for a fuel cell and a preparation method and application thereof. The preparation method comprises the following steps: (1) grinding and mixing raw materials including a platinum carbon catalyst, an ionomer, a composite solvent, a photoinitiator, and an α-olefin sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) coating the catalyst slurry on a base film PET or a proton exchange membrane, and irradiating the first time with ultraviolet light to obtain an initial solidified layer; (3) heat treatment in stages, wherein the first stage is heating at normal pressure at a temperature of 85-95°C; the second stage is vacuum heating at a temperature of 100-105°C, a vacuum degree of 0.5Mpa, and a time of 1-2h; the third stage is vacuum heating at a temperature of 115-120°C, a vacuum degree of 0.5Mpa, and a time of 1-2h; (4) cooling to room temperature, and irradiating the second time with ultraviolet light for 1-2h to obtain a catalyst layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen fuel cells, and in particular to an anode catalyst layer for a fuel cell, a preparation method thereof and an application thereof. Background Art

[0002] The most important part of a hydrogen fuel cell is the catalyst. The catalytic efficiency of the catalyst directly determines the power of the entire fuel cell; at the same time, the amount of platinum (Pt) in the catalyst also plays an important role in the cost of the entire fuel cell. In fact, the distribution of Pt in the fuel cell is uneven (8 / 9 of the Pt / C catalyst is distributed at the positive electrode of the fuel cell). This is because in a hydrogen fuel cell, the HOR reaction H2→2e - +2H + (Two electron transfer, fast kinetic process), ORR reaction O2+4e occurs at the positive electrode - +4H + →2H2O (four electron transfer, slow kinetics). According to theoretical calculations and comparison of the two reaction kinetics, the ORR reaction rate at the positive electrode is 6 orders of magnitude lower than the HOR reaction at the negative electrode, so the reaction rate of the overall reaction depends on the positive electrode. The chemical reaction rate is proportional to the amount of Pt catalyst used, so the amount of catalyst used at the positive electrode is about 8 times that of the negative electrode.

[0003] The catalyst Pt / C is made of ionomers adhered between the proton exchange membrane (PEM) and the gas diffusion layer (GDL). The surface of the catalyst Pt is wrapped by the ionomer, and oxygen must first permeate through the ionomer before it can contact the catalyst Pt, thereby triggering the ORR reaction. The catalyst layer is the place where the electrochemical reaction occurs inside the fuel cell, where the transfer of protons and electrons, as well as the transfer of the reaction gas and the product water gas-liquid two-phase flow occur. Therefore, how to improve the transfer efficiency of protons, electrons, and oxygen in the catalyst layer and improve the catalytic efficiency of the catalyst is the main research direction. Summary of the invention

[0004] In view of the problems existing in the background technology, the purpose of the present invention is to provide an anode catalyst layer for a fuel cell and a preparation method and application thereof. The catalyst layer prepared by this method has good diffusion capacity of protons, reaction gases and water, and the catalytic efficiency is significantly improved.

[0005] In order to achieve the above-mentioned object, the present invention provides a method for preparing an anode catalyst layer for a fuel cell, which comprises the following steps: (1) grinding and mixing raw materials including a platinum carbon catalyst, an ionomer, a composite solvent, a photoinitiator, and an α-olefin sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) coating the catalyst slurry on a base film PET or a proton exchange membrane, irradiating the first time with ultraviolet light for 1-2 hours, and obtaining an initial cured layer; (3) performing a heat treatment in stages, wherein the first stage is heating at normal pressure at a temperature of 85-95°C for 1-2 hours; the second stage is vacuum heating at a temperature of 100-105°C, a vacuum degree of 0.5Mpa, and a time of 1-2 hours; the third stage is vacuum heating at a temperature of 115-120°C, a vacuum degree of 0.5Mpa, and a time of 1-2 hours; (4) cooling to room temperature, irradiating the second time with ultraviolet light for 1-2 hours, and obtaining a catalyst layer; the mass ratio of the platinum carbon catalyst, the ionomer, the composite solvent, the photoinitiator, and the α-olefin sulfonic acid is 3-8:10-20:50-60: 0.02-0.05:0.8-1; the ionomer is one or a combination of poly (PDD-co-PSVE) and poly (TFE-PDD-PSVE); the composite solvent is composed of deionized water, ethanol and isobutyl alcohol in a mass ratio of 1:1:1; the photoinitiator is perfluorooctanoic acid-2-[4-(2-hydroxy-2-methylpropionyl)phenoxy]ethyl ester; the α-olefin sulfonic acid is C 14 -C 16 α-olefins are obtained by sulfonation with SO3.

[0006] Optionally, the platinum-carbon catalyst is one or a combination of a carbon-supported Pt catalyst, a carbon-supported Pt alloy catalyst, and a carbon-supported Pt monolayer catalyst.

[0007] The present invention also provides an anode catalyst layer for a fuel cell prepared by the method for preparing an anode catalyst layer for a fuel cell as described above.

[0008] The present invention also provides an application of the anode catalyst layer for a fuel cell as described above, which is applied to a hydrogen fuel cell.

[0009] The beneficial effects of the present invention are as follows:

[0010] 1. The photoinitiator and α-olefin sulfonic acid in the catalyst slurry undergo cross-linking or grafting reactions inside and on the interface of the slurry under the action of ultraviolet light, which significantly increases the viscosity of the coated catalyst slurry and forms a gel-like film layer; then, after three normal pressure heat treatment stages at different temperatures and a vacuum heat treatment stage, solvents such as water, ethanol and isopropanol with different boiling points or volatilities are removed in turn, and the gel-like catalyst film layer becomes a catalyst layer with multi-dimensional pores.

[0011] 2. The catalyst layer prepared by this method has good diffusion capacity for protons, reaction gases and water, and the catalytic efficiency is significantly improved. DETAILED DESCRIPTION

[0012] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.

[0013] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0014] According to the present invention, the anode catalyst layer for a fuel cell comprises a platinum-carbon catalyst, an ionomer, a composite solvent, a photoinitiator and an α-olefin sulfonic acid; the composite solvent is composed of deionized water, ethanol and isobutyl alcohol in a mass ratio of 1:1:1. The platinum-carbon catalyst can be one or a combination of a carbon-supported Pt catalyst, a carbon-supported Pt alloy catalyst and a carbon-supported Pt monolayer catalyst. The α-olefin sulfonic acid can be C 14 -C 16 The ionomer can be one or a combination of poly(PDD-co-PSVE) and poly(TFE-PDD-PSVE).

[0015] In the anode catalyst layer for a fuel cell according to the present invention, the mass ratio of the platinum-carbon catalyst, the ionomer, the composite solvent, the photoinitiator, and the α-olefin sulfonic acid may be 3-8:10-20:50-60:0.02-0.05:0.8-1.

[0016] In the anode catalyst layer for a fuel cell according to the present invention, the photoinitiator may be 2-[4-(2-hydroxy-2-methylpropionyl)phenoxy]ethyl perfluorooctanoate.

[0017] The method for preparing an anode catalyst layer for a fuel cell according to the present invention comprises the following steps: (1) grinding and mixing raw materials including a platinum carbon catalyst, an ionomer, a composite solvent, a photoinitiator, and an α-olefin sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) coating the catalyst slurry on a base film PET or a proton exchange membrane, irradiating the base film with ultraviolet light for a first time for 1-2 hours to obtain an initial cured layer; (3) performing a heat treatment in stages, wherein the first stage is heating at normal pressure at a temperature of 85-95° C. for 1-2 hours; the second stage is vacuum heating at a temperature of 100-105° C., a vacuum degree of 0.5 MPa, and a time of 1-2 hours; the third stage is vacuum heating at a temperature of 115-120° C., a vacuum degree of 0.5 MPa, and a time of 1-2 hours; and (4) cooling to room temperature and irradiating the base film with ultraviolet light for a second time for 1-2 hours to obtain a catalyst layer.

[0018] The anode catalyst layer for a fuel cell according to the present invention can be applied to a hydrogen fuel cell.

[0019] The anode catalyst layer for fuel cells of the present invention and its preparation method and application are described in detail below through examples. Main raw materials and equipment used: Unless otherwise specified, the raw materials and equipment of each embodiment and comparative example are the same; materials without specific models or types are from the same common models purchased on the market, and no specific restrictions are imposed.

[0020] Raw materials:

[0021] Pt / C catalyst, TEC10E40E, TANAKA, Japan;

[0022] poly (PDD-co-PSVE), Toyota, Japan;

[0023] Perfluorooctanoic acid-2-[4-(2-hydroxy-2-methylpropionyl)phenoxy]ethyl ester, homemade, the specific synthesis method is based on the literature ("Synthesis and Performance Study of Fluorinated Photoinitiators", Yu Yunyingdeng, "Imaging Science and Photochemistry", Vol. 31, No. 6, pp. 448-459, November 2013);

[0024] α-Olefin sulfonic acid, homemade: C 14 -C 16 The α-olefin is reacted with 10% sulfur trioxide in a falling film continuous sulfonation reactor, the product is hydrolyzed, allowed to stand for stratification, and the oil phase is dried to obtain α-olefin sulfonic acid.

[0025] Example 1

[0026] (1) 3 g of Pt / C catalyst (carbon-supported Pt catalyst), 10 g of poly (PDD-co-PSVE), 50 g of composite solvent, 0.02 g of perfluorooctanoic acid-2-[4-(2-hydroxy-2-methylpropionyl)phenoxy]ethyl ester, and 0.8 g of α-olefin sulfonic acid are ground and mixed uniformly in a grinding mixer at room temperature to obtain a catalyst slurry; the composite solvent is composed of deionized water, ethanol and isobutanol in a mass ratio of 1:1:1; (2) the catalyst slurry is coated on a base film PET or a proton exchange membrane, and the first ultraviolet light irradiation of a high-pressure mercury lamp, 100 w / m 2 , time 1h, to obtain the initial solidified layer; (3) heat treatment in stages, the first stage is heating at normal pressure, temperature 85℃, time 1h; the second stage is vacuum heating, temperature 100℃, vacuum degree 0.5Mpa, time 1h; the third stage is vacuum heating, temperature 115℃, vacuum degree 0.5Mpa, time 1h; (4) cooling to room temperature, second ultraviolet irradiation with high pressure mercury lamp, 100w / m 2 , time 1h, to obtain a catalyst layer.

[0027] Example 2

[0028] (1) 8 g of Pt / C catalyst, 20 g of poly (PDD-co-PSVE), 60 g of composite solvent, 0.05 g of perfluorooctanoic acid-2-[4-(2-hydroxy-2-methylpropionyl)phenoxy]ethyl ester, and 1 g of α-olefin sulfonic acid are ground and mixed uniformly in a grinding mixer at room temperature to obtain a catalyst slurry; the composite solvent is composed of deionized water, ethanol and isobutanol in a mass ratio of 1:1:1; (2) the catalyst slurry is coated on a base film PET or a proton exchange membrane, and the first ultraviolet light irradiation of a high-pressure mercury lamp, 100 w / m 2 , time 2h, to obtain the initial solidified layer; (3) heat treatment in stages, the first stage is heating at normal pressure, temperature 95℃, time 2h; the second stage is vacuum heating, temperature 105℃, vacuum degree 0.5Mpa, time 2h; the third stage is vacuum heating, temperature 120℃, vacuum degree 0.5Mpa, time 2h; (4) cooling to room temperature, second ultraviolet irradiation with high pressure mercury lamp, 100w / m 2 , time 2h, to obtain a catalyst layer.

[0029] Example 3

[0030] (1) 6 g of Pt / C catalyst, 15 g of poly (PDD-co-PSVE), 55 g of composite solvent, 0.03 g of perfluorooctanoic acid-2-[4-(2-hydroxy-2-methylpropionyl)phenoxy]ethyl ester, and 0.9 g of α-olefin sulfonic acid are ground and mixed uniformly in a grinding mixer at room temperature to obtain a catalyst slurry; the composite solvent is composed of deionized water, ethanol and isobutanol in a mass ratio of 1:1:1; (2) the catalyst slurry is coated on a base film PET or a proton exchange membrane, and the first ultraviolet light irradiation of a high-pressure mercury lamp, 100 w / m 2 , time 1.5h, to obtain the initial solidified layer; (3) heat treatment in stages, the first stage is heating at normal pressure, temperature 90℃, time 1.5h; the second stage is vacuum heating, temperature 103℃, vacuum degree 0.5Mpa, time 1.5h; the third stage is vacuum heating, temperature 118℃, vacuum degree 0.5Mpa, time 1.5h; (4) cooling to room temperature, second ultraviolet irradiation with high pressure mercury lamp, 100w / m 2 , time 1.5h, to obtain a catalyst layer.

[0031] Comparative Example 1

[0032] Except that the photoinitiator and α-olefin sulfonic acid were not used, the other steps were the same as those in Example 3.

[0033] Comparative Example 2

[0034] Except that the composite solvent is replaced by deionized water, other aspects are the same as those in Example 3.

[0035] Performance Testing

[0036] 1. The thickness of the catalyst layer in the examples and comparative examples was 0.2 mm.

[0037] 2. At 23°C and 0% relative humidity, the oxygen permeability of the catalyst layer after peeling off from the surface of the base membrane PET was tested using an instrument (Mocon OX-Tran®, Minneapolis, MN, USA); at 80°C and 95% relative humidity, the catalyst layer was loaded into the electrolyte membrane of the electrochemical cell, the test electrodes were connected to both sides of the electrolyte membrane, an external voltage was applied, and the proton conductivity was calculated.

[0038] 3. The mechanical strength and interlayer peel strength of the composite membrane composed of the catalyst layer and the proton exchange membrane (perfluorosulfonic acid ion membrane, N117, Nafion, DuPont, USA) were tested using a universal material testing machine (GB / T 20042.3-2022).

[0039] See Table 1 for specific data.

[0040] Table 1

[0041]

[0042] It can be seen from the data of the examples and comparative examples that the photocuring viscosity enhancement structure used in the preparation method of the present invention provides a prerequisite for subsequent solvent pore formation, and the obtained catalyst layer has multi-dimensional pores, good oxygen permeability and proton conductivity, and fully exerts the catalytic efficiency of the catalyst layer. The strength and interlayer peeling strength of the composite membrane composed of the catalyst layer and the proton exchange membrane are also significantly improved.

[0043] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing an anode catalyst layer for a fuel cell, characterized in that: The method comprises the following steps: (1) grinding and mixing raw materials including a platinum carbon catalyst, an ionomer, a composite solvent, a photoinitiator and an α-olefin sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) coating the catalyst slurry on a base film PET or a proton exchange membrane, irradiating the base film with ultraviolet light for a first time for 1-2 hours to obtain a primary solidified layer; (3) performing a heat treatment in stages, wherein the first stage is heating at normal pressure at a temperature of 85-95° C. for a time of 1-2 hours; the second stage is vacuum heating at a temperature of 100-105° C., a vacuum degree of 0.5 Mpa for a time of 1-2 hours; the third stage is vacuum heating at a temperature of 115-120° C., a vacuum degree of 0.5 Mpa for a time of 1-2 hours; (4) cooling to room temperature, irradiating the base film with ultraviolet light for a second time for 1-2 hours to obtain a catalyst layer; The mass ratio of the platinum-carbon catalyst, ionomer, composite solvent, photoinitiator, and α-olefin sulfonic acid is 3-8:10-20:50-60:0.02-0.05:0.8-1; the ionomer is one or a combination of poly(PDD-co-PSVE) and poly(TFE-PDD-PSVE); the composite solvent is composed of deionized water, ethanol, and isobutyl alcohol in a mass ratio of 1:1:1; the photoinitiator is perfluorooctanoic acid-2-[4-(2-hydroxy-2-methylpropionyl)phenoxy]ethyl ester; the α-olefin sulfonic acid is C 14 -C 16 It is obtained by sulfonation of α-olefins with SO3.

2. The method for preparing an anode catalyst layer for a fuel cell according to claim 1, wherein: The platinum-carbon catalyst is one or a combination of a carbon-supported Pt catalyst, a carbon-supported Pt alloy catalyst, and a carbon-supported Pt single-layer catalyst.

3. An anode catalyst layer for a fuel cell prepared by the method for preparing an anode catalyst layer for a fuel cell according to any one of claims 1 to 2.

4. The use of the anode catalyst layer for a fuel cell according to claim 3, characterized in that: Used in hydrogen fuel cells.