A high loading FeO x Preparation method and application of nanocluster / nitrogen-doped biochar

By preparing FeOx nanoclusters/nitrogen doped biocarbons on a nitrogen-doped biocarbon support with high specific surface area, the problems of limited performance of hydrogen peroxide catalysts and difficulty in preparing nanoclusters are solved, and efficient catalytic oxidation reactions and pollutant removal are achieved, satisfying the satisfaction of Strict emission standards.

CN118698587BActive Publication Date: 2024-11-26SUN YAT SEN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196650.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-26
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

In the existing advanced oxidation technology, the catalytic performance of hydrogen peroxide catalysts is limited, and the preparation of metal oxide nanoclusters is difficult, especially the randomness and instability supported on the support lead to low catalytic activity.

Method used

Using ultra-high specific surface area doped nitrogen biocarbon as a carrier, the Fe-N5 structure is formed by axial coordination between iron phthalocyanine (II) and its axial coordination, inhibiting the agglomeration of iron phthalocyanine (II), and preparing a high load and small particle size. FeOx nanoclusters/nitrogen doped biocarbons are used in hydrogen peroxide catalysts to promote the decomposition of oxidants to produce reactive oxygen species.

Benefits of technology

A highly efficient catalytic oxidation reaction was achieved, especially the removal rates of chlorophenol compounds, antibiotics and dyes exceeded 90%, and the removal effect of more than 98% in the ozone peroxidation reaction was achieved, meeting the emission standards of electroplating pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118698587B_ABST
    Figure CN118698587B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of catalyst materials, and particularly relates to a high-load FeO x Preparation method and application of nanocluster / nitrogen-doped biochar. x Nanocluster / nitrogen-doped biochar is a carbon with ultra-high specific surface area (≥2000 m 2 / g) and biochar rich in N doping (N content ≥ 3.0%) was used as a carrier, impregnated with iron phthalocyanine (II) and stirred and evaporated to dryness, and then pyrolyzed under an inert atmosphere to obtain FeO with high metal loading. x Nanocluster / nitrogen-doped biochar. The FeO x The preparation process of nanocluster / nitrogen-doped biochar is simple and controllable, and it has excellent catalytic H 2 O 2 (Fenton-like) and catalytic H 2 O 2 / O 3 (Ozone peroxidation) performance, which can achieve efficient degradation of difficult-to-degrade pollutants including dyes, antibiotics, chlorophenols, and nickel-containing organic complexes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst materials. More specifically, it relates to a high-load FeO x Preparation methods and applications of nanocluster / nitrogen-doped biochar. Background Art

[0002] With the rapid development of global industry, various wastewaters containing difficult-to-degrade pollutants have been produced. Advanced oxidation technology is one of the main ways to treat wastewater. There are many types of advanced oxidation technologies, which mainly use oxidants such as hydrogen peroxide, ozone, persulfate, oxygen, etc. to produce other active species such as hydroxyl radicals under external conditions such as light, catalysts, electrochemistry, heating and pressure, and strong alkali to degrade organic matter, thereby achieving the purpose of wastewater treatment.

[0003] At present, advanced oxidation technology mainly uses hydrogen peroxide and ozone as oxidants. Under the condition of hydrogen peroxide catalyst, H2O2 is catalyzed to form Fenton-like catalytic oxidation technology, or O3 / H2O2 is catalyzed to form catalytic ozone peroxidation technology; under the action of hydrogen peroxide catalyst, H2O2 or O3 / H2O2 quickly decomposes to produce various active oxygen species (such as hydroxyl radicals, singlet oxygen, surface oxygen atoms, etc.), which can effectively degrade those highly stable and difficult to degrade organic pollutants, thereby achieving deep oxidation and maximizing the removal of organic pollutants. For example, Chinese patent application CN 114100650A proposes an ozone-hydrogen peroxide catalytic oxidation catalyst. Under the conditions of ozone and hydrogen peroxide (oxidant), a catalyst is added to promote the decomposition of the oxidant to produce hydroxyl radicals, and degrade organic matter in biochemical wastewater, but its preparation method is complicated, requires the use of multiple metals in combination, and has limited catalytic performance.

[0004] Nanoclusters refer to structures between single atoms and nanoparticles that are assembled from a few atoms. Compared with single atoms, nanoclusters are easier to prepare, and the atoms in nanoclusters may have mixed valence states, which is more conducive to the redox reaction of the catalyst in the catalytic reaction; compared with nanoparticles, nanoclusters have more exposed atoms, and these exposed atoms have no atoms in the outer layer to coordinate with them, so they have dangling bonds (unsaturated coordination) and show significant interface effects and size effects, thus having ultra-high catalytic activity. However, due to the high surface energy and thermodynamic instability of nanoclusters, the preparation of existing technologies is still difficult, especially the preparation of nanoclusters of metal oxides, which are usually loaded on porous carriers. However, this load has no fixed riveting points and is random, and is very easy to aggregate to form large particles of metal oxides rather than clusters. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art hydrogen peroxide catalyst, such as limited catalytic performance and difficulty in preparing metal oxide nanoclusters, and to provide a FeO x Preparation method of nanocluster / nitrogen-doped biochar.

[0006] The purpose of the present invention is to provide a FeO x Nanocluster / nitrogen-doped biochar.

[0007] Another object of the present invention is to provide the FeO x Application of nanocluster / nitrogen-doped biochar as hydrogen peroxide catalyst.

[0008] Another object of the present invention is to provide the FeO x Application of nanocluster / nitrogen-doped biochar in the degradation of organic pollutants.

[0009] The above-mentioned purpose of the present invention is achieved through the following solutions:

[0010] The present invention provides a FeO x The method for preparing nanocluster / nitrogen-doped biochar comprises the following steps:

[0011] S1. placing the nitrogen-doped biocarbon carrier in an iron (II) phthalocyanine solution, immersing and evaporating at 40-60°C to obtain a precursor;

[0012] S3. Take the precursor described in S1 and pyrolyze it at 700-900°C under an inert atmosphere, and then post-treat it to obtain FeO x Nanoclusters / nitrogen-doped biochar;

[0013] The mass volume ratio of the nitrogen-doped biocarbon carrier to the iron (II) phthalocyanine solution is 4.0-5.8 g:1L;

[0014] The specific surface area of ​​the nitrogen-doped biocarbon carrier is ≥ 2000 m 2 / g, and N content ≥3.0%.

[0015] The invention adopts nitrogen-doped biochar with ultra-high specific surface area as a carrier, and uses iron phthalocyanine (II) as an iron source and a partial nitrogen source. The abundant nitrogen doping on the surface of the carrier can serve as an active anchor point of iron phthalocyanine (II), and form axially coordinated Fe-N5 with the Fe-N4 plane structure in iron phthalocyanine (II), so as to anchor iron phthalocyanine (II) on the surface of the biochar carrier, thereby inhibiting the aggregation of iron phthalocyanine (II) during the pyrolysis process. After pyrolysis, FeO x Nanocluster / nitrogen-doped biochar has the advantages of high metal loading, extremely small particle size and high metal dispersion. xNanoclusters / nitrogen-doped biochar also contain abundant Fe-N groups, which can promote the electron transport of the catalyst, thereby more efficiently catalyzing oxidants (such as one or more of hydrogen peroxide and ozone) to produce reactive oxygen species and improving the catalytic activity.

[0016] In the present invention, the temperature of the impregnation evaporation is 40-60° C. If the temperature is too low, the iron phthalocyanine (II) solid may precipitate, cannot be evenly loaded, and will cause the evaporation time to be too long; if the temperature is too high, the solvent evaporates quickly, which is not conducive to the uniform dispersion and anchoring of iron phthalocyanine (II) on the carrier surface.

[0017] In the present invention, the mass volume ratio of the nitrogen-doped biocarbon carrier to the iron phthalocyanine (II) solution is 4.0-5.8 g: 1 L. If the mass volume ratio is too high, the iron loading will be too low, which is not conducive to the impregnation mass transfer process, and even the iron phthalocyanine (II) solution cannot immerse the biocarbon carrier; if the mass volume ratio is too low, the iron loading will be too high, and the iron element will agglomerate severely during the pyrolysis process, and only low-activity FeO can be generated. x Large particles cannot produce highly active FeO x Nanoclusters will not only cause solvent waste, but also increase the subsequent evaporation time.

[0018] In the present invention, if the specific surface area of ​​the nitrogen-doped biocarbon carrier is too low and the N content is too low, the iron phthalocyanine (II) cannot be evenly anchored on the carrier surface, and metal agglomeration is likely to occur during the heat treatment process, forming large particles of FeO x , resulting in clogging of the carrier pores, which in turn inhibits the mass transfer of reactants and reduces catalytic activity. In addition, metal agglomerates to form large particles of FeO x After that, the prepared FeO x Nanocluster / nitrogen-doped biochar cannot obtain abundant Fe-N5 groups, which leads to poor conductivity and is not conducive to redox electron transfer in catalytic reactions. 2 / g and N content ≥3.0%, the technical effect claimed by the present invention can be achieved, and the larger the specific surface area and the higher the N content, the better the final effect.

[0019] In the pyrolysis process of the preparation method of the present invention, if the pyrolysis temperature is too low, the pyrolysis conversion of iron phthalocyanine (II) cannot be complete; if the pyrolysis temperature is too high, FeO x Nanoclusters are prone to agglomeration, and the pore structure in the carrier biochar is prone to collapse, which is not conducive to subsequent catalytic reactions.

[0020] Preferably, the mass volume ratio of the nitrogen-doped biocarbon carrier to the iron (II) phthalocyanine solution is 4.5-5.5 g:1L.

[0021] Furthermore, in the FeO x In the preparation method of nanocluster / nitrogen-doped biochar, the solvent in the iron (II) phthalocyanine solution is a mixed solution of ethanol and tetrahydrofuran in a volume ratio of 1:0.8-1.2.

[0022] Furthermore, in the FeO x In the method for preparing nanocluster / nitrogen-doped biochar, the concentration of phthalocyanine iron (II) in the phthalocyanine iron (II) solution is 2.0-3.0 g / L. When the concentration of phthalocyanine iron (II) in the phthalocyanine iron (II) solution of the present invention is within the above range, phthalocyanine iron (II) is more easily dissolved in the solvent, which is beneficial for subsequent impregnation dispersion and drying, so that the prepared FeO x Nanoclusters / nitrogen-doped biochar have better catalytic effect.

[0023] Preferably, the concentration of the iron phthalocyanine (II) is 2.2-2.8 g / L; more preferably, the concentration of the iron phthalocyanine (II) is 2.4-2.6 g / L.

[0024] Furthermore, the inert atmosphere is nitrogen or argon; most preferably, it is nitrogen.

[0025] Furthermore, the heating rate of the pyrolysis is 3-10 °C / min. Within this heating rate range, iron phthalocyanine (II) is not easy to decompose too quickly, and the subsequent surface FeO x Nanoclusters can be fully dispersed, exposing more active sites, which is more conducive to subsequent catalytic reactions.

[0026] Furthermore, the pyrolysis time is 1 to 4 h. Within this range, the FeO prepared by pyrolysis x Nanocluster / nitrogen-doped biochar has better catalytic performance.

[0027] Furthermore, the post-treatment is cooling to room temperature, washing with water until neutral, drying, and grinding.

[0028] Furthermore, in the FeO x In the method for preparing nanocluster / nitrogen-doped biochar, the nitrogen-doped biochar carrier is obtained by modifying biochar by nitrogen doping, and can be purchased commercially or prepared according to the method of the present invention.

[0029] For reference, the present invention provides a method for preparing a nitrogen-doped biocarbon carrier:

[0030] S11. Mix the biomass raw material and zinc chloride in water at a mass ratio of 1:(0.8-1.2), dry, and then calcine at 480-520° C. under an inert atmosphere, wash, and dry to obtain a solid;

[0031] S12. The solid prepared in S11 is mixed with KOH in a mass ratio of 1:(1.5-2.5), calcined at 800-900°C under an inert atmosphere, and post-treated to obtain biochar;

[0032] S13. The biochar prepared in S12 is mixed with urea in a mass ratio of 1:(0.8-1.4), calcined at 330-370° C. under an inert atmosphere, and post-treated to obtain a nitrogen-doped biochar carrier.

[0033] Furthermore, the biomass raw material is one or more of wheat bran, rice husk, bean dregs, leaves, and straw.

[0034] Furthermore, in step S11, the concentration of zinc chloride in the water is 150.0-250.0 g / L.

[0035] Furthermore, in step S11, the mixing needs to be stirred for 10 to 30 minutes.

[0036] Furthermore, the calcination is performed at a heating rate of 5 to 15 °C / min.

[0037] Furthermore, in step S11, the calcination time is 0.8-1.2 h.

[0038] Furthermore, in steps S12 and S13, the calcination time is 1.5 to 2.5 h.

[0039] The present invention also protects the FeO prepared by the preparation method. x Nanocluster / nitrogen-doped biochar.

[0040] The present invention protects the FeO x Application of nanocluster / nitrogen-doped biochar as hydrogen peroxide catalyst.

[0041] The FeO of the present invention x Nanoclusters / nitrogen-doped biochar as hydrogen peroxide catalysts can catalyze H2O2 alone (Fenton-like oxidation reaction) or catalyze O3 / H2O2 (ozone peroxidation reaction) to degrade organic pollutants in water.

[0042] Specifically, in the effect examples of the present invention, the FeO prepared in the examples x Nanocluster / nitrogen-doped biochar catalyzes Fenton-like oxidation reactions, which can effectively degrade chlorophenol compounds, antibiotic pollutants or dyes. More specifically, the removal rate of 2,4,6-trichlorophenol reached 91.5%, the removal rate of antibiotic pollutant sulfamethoxazole reached 92.3%, and the removal rate of dye acid orange 7 reached 90.8%.

[0043] In addition, the FeO prepared by the preparation method of the present invention x Nanocluster / nitrogen-doped biochar also showed good removal effect on EDTA-Ni organic complex. In the ozone peroxidation catalytic oxidation reaction, Ni 2+ The concentration is below the detection limit and meets the emission standard (<0.1 mg / L) specified in the "Emission Standard of Electroplating Pollutants" (GB21900-2008).

[0044] Additionally, the present invention protects the FeO x Application of nanocluster / nitrogen-doped biochar in the degradation of organic pollutants.

[0045] Furthermore, the organic pollutants include but are not limited to dyes, antibiotics, chlorinated phenol compounds, nickel-containing organic complexes and other difficult-to-degrade organic substances.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The FeO of the present invention x Nanocluster / nitrogen-doped biochar uses nitrogen-doped biochar with ultra-high specific surface area as a carrier. The abundant doped nitrogen on the carrier surface can serve as an active anchor point for phthalocyanine iron (II), forming an axially coordinated Fe-N5 with the Fe-N4 planar structure in phthalocyanine iron (II), anchoring phthalocyanine iron (II) on the surface of the biochar carrier, thereby inhibiting the aggregation of phthalocyanine iron (II) during pyrolysis. After pyrolysis, FeO with high loading, extremely small particle size (<6 nm) and high dispersion can be prepared. x Nanoclusters are catalytically active centers. In addition, FeO x Nanoclusters / nitrogen-doped biochar can be used as hydrogen peroxide catalysts to degrade organic pollutants in water by catalyzing H2O2 alone (Fenton-like oxidation reaction) or catalyzing O3 / H2O2 (ozone peroxidation reaction). x Nanocluster / nitrogen-doped biochar contains abundant Fe-N groups, which can promote the electron transfer of the catalyst and improve the catalytic activity of the catalyst, making its removal effect on chlorophenol compounds, antibiotics, and dyes greater than 90%; the removal rate of nickel-containing organic complexes is above 98%. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 The electron microscope image and element distribution map of the product prepared in Example 1. DETAILED DESCRIPTION

[0049] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0050] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0051] Example 1

[0052] The specific preparation method of the nitrogen-doped biocarbon carrier in this embodiment is as follows:

[0053] S11. The washed and dried wheat bran biomass raw material was crushed and passed through a 0.3 mm sieve to obtain biomass powder, and then added to a certain volume of zinc chloride aqueous solution at a mass ratio of biomass powder to zinc chloride of 1:1, wherein the concentration of zinc chloride in the zinc chloride aqueous solution was 200.0 g / L. After stirring for 20 minutes, the mixture was dried in an oven at 105°C. The dried solid was placed in a tubular furnace and pyrolyzed and carbonized under nitrogen protection (heating to 500°C at a heating rate of 10°C / min and pyrolyzed for 1.0 h). After cooling to room temperature, the mixture was washed with dilute hydrochloric acid and pure water for several times until the solution was neutral, and the solid material was obtained by centrifugation, and then dried in an oven at 105°C to obtain a solid.

[0054] S12. The dried solid of S11 was ground and mixed with KOH in a mass ratio of 1:2, and then placed in a tube furnace for pyrolysis and carbonization under nitrogen protection (heating to 900°C at a rate of 10°C / min and pyrolysis for 2 h), cooled to room temperature, washed with dilute hydrochloric acid and pure water several times until the solution was neutral, centrifuged to obtain a solid material, dried in an oven, and ground through a 200-mesh sieve to obtain biochar;

[0055] S13. The biochar after sieving S12 was ground and mixed with urea in a mass ratio of 1:1, and then placed in a tubular furnace for pyrolysis and nitrogen doping under nitrogen protection (heating to 350°C at a rate of 5°C / min, pyrolysis for 2 h), cooled to room temperature, washed with pure water several times until the solution was neutral, centrifuged to obtain a solid material, dried in an oven at 105°C, and ground through a 200-mesh sieve to obtain a nitrogen-doped biochar carrier;

[0056] The specific surface area of ​​the nitrogen-doped biocarbon carrier is 2648.6 m 2 / g, and the nitrogen content is 3.5%.

[0057] A FeO x Nanocluster / nitrogen-doped biochar, the preparation process is as follows:

[0058] S1. Dissolve 0.05 g of phthalocyanine iron (II) in a mixed solution of 10 mL of ethanol and 10 mL of tetrahydrofuran, and stir until the phthalocyanine iron (II) is completely dissolved (about 10 min). At this time, the concentration of phthalocyanine iron (II) is 2.5 g / L; add 100 mg of the nitrogen-doped biocarbon carrier prepared above to the above phthalocyanine iron (II) solution. At this time, the mass volume ratio of the biocarbon carrier to the phthalocyanine iron (II) solution is 5.0 g: 1L, stir for 3 h, mix thoroughly, immerse and stir at a constant temperature of 60°C and evaporate to dryness to obtain a precursor;

[0059] S2. The precursor of S1 was placed in a tube furnace, heated to 800°C at a rate of 5°C / min in an Ar atmosphere, pyrolyzed at 800°C for 2 h, cooled to room temperature, washed with water until neutral, dried, and ground to obtain FeO x Nanocluster / nitrogen-doped biochar, the theoretical iron content is about 4.7%.

[0060] The final product was prepared by scanning electron microscopy. Figure 1 As shown, from Figure 1 The electron microscope image on the left shows FeO x Nanocluster / nitrogen-doped biochar has a porous structure and FeO x The iron elements on the surface of nanocluster / nitrogen-doped biochar are mainly iron oxide nanoclusters with an average particle size of <6 nm; Figure 1 From the element distribution diagram on the right, we can see that FeO x The distribution areas of Fe, N and Fe, O elements in nanocluster / nitrogen-doped biochar are highly overlapped and evenly distributed. According to the synthesis conditions, XRD, N2 adsorption-desorption curve analysis, and XPS, it can be known that FeO x The surface of nanocluster / nitrogen-doped biochar also contains abundant Fe-N5 functional groups. x The specific surface area of ​​nanocluster / nitrogen-doped biochar is still as high as 1650.7 m 2 / g.

[0061] Example 2

[0062] The specific preparation method of the nitrogen-doped biocarbon carrier in this embodiment is as follows:

[0063] S11. The washed and dried bean dregs biomass raw material was crushed and passed through a 0.3 mm sieve to obtain biomass powder, and the biomass powder was added to a certain volume of zinc chloride aqueous solution at a mass ratio of 1:1 to zinc chloride, wherein the concentration of zinc chloride in the zinc chloride aqueous solution was 150.0 g / L. After stirring for 15 minutes, the mixture was dried in an oven at 105°C. The dried solid was placed in a tubular furnace for pyrolysis and carbonization under nitrogen protection (after heating to 500°C at a rate of 10°C / min, pyrolysis was performed for 0.8 h). After cooling to room temperature, the mixture was washed with dilute hydrochloric acid and pure water for several times until the solution was neutral, and the solid material was obtained by centrifugation, and dried in an oven at 105°C to obtain a solid.

[0064] S12. The dried solid of S11 was ground and mixed with KOH in a mass ratio of 1:2, and then placed in a tubular furnace for pyrolysis and carbonization under nitrogen protection (heating rate of 10 °C / min to 800 °C, pyrolysis for 2.5 h), cooled to room temperature, washed with dilute hydrochloric acid and pure water several times until the solution was neutral, centrifuged to obtain a solid material, dried in an oven, and ground through a 200-mesh sieve to obtain biochar;

[0065] S13. The biochar after screening S12 was ground and mixed with urea in a mass ratio of 1:0.8, and then placed in a tubular furnace for pyrolysis and nitrogen doping under argon protection (heating rate of 5 °C / min to 350 °C, pyrolysis for 2 h), cooled to room temperature, washed with pure water several times until the solution was neutral, centrifuged to obtain a solid material, dried in an oven at 105 °C, and ground through a 200-mesh sieve to obtain a nitrogen-doped biochar carrier;

[0066] The specific surface area of ​​the nitrogen-doped biocarbon carrier is 2123.2 m 2 / g, and the nitrogen content is 3.1%.

[0067] A FeO x Nanocluster / nitrogen-doped biochar, the preparation process is as follows:

[0068] S1. Dissolve 0.04 g of phthalocyanine iron (II) in a mixed solution of 10 mL of ethanol and 10 mL of tetrahydrofuran, and stir until the phthalocyanine iron (II) is completely dissolved (about 10 min). At this time, the concentration of phthalocyanine iron (II) is 2 g / L; add 116 mg of the nitrogen-doped biocarbon carrier prepared above to the above phthalocyanine iron (II) solution. At this time, the volume ratio of the biocarbon carrier mass to the phthalocyanine iron (II) solution is 5.8 g: 1L, stir for 3 h, mix thoroughly, and evaporate to dryness at a constant temperature of 60°C with stirring to obtain a precursor;

[0069] S2. The precursor of S1 was placed in a tube furnace, heated to 700°C at a rate of 5°C / min in N2, pyrolyzed at 700°C for 4 h, cooled to room temperature, washed with water until neutral, dried, and ground to obtain FeO x Nanocluster / nitrogen-doped biochar, the theoretical iron content is about 3.3% by mass.

[0070] Example 3

[0071] The specific preparation method of the nitrogen-doped biocarbon carrier in this embodiment is as follows:

[0072] S11. The washed and dried leaf biomass raw material was crushed and passed through a 0.3 mm sieve to obtain biomass powder, and then added to a certain volume of zinc chloride aqueous solution according to a mass ratio of biomass powder to zinc chloride of 1:1.2, wherein the concentration of zinc chloride in the zinc chloride aqueous solution was 250.0 g / L. After stirring for 30 minutes, the dried material was dried in an oven at 105°C, and the dried solid was placed in a tubular furnace for pyrolysis and carbonization under argon protection (after heating to 500°C at a rate of 10°C / min, pyrolysis for 1.2 hours), cooled to room temperature, washed with dilute hydrochloric acid and pure water several times until the solution was neutral, centrifuged to obtain a solid material, and dried in an oven at 105°C to obtain a solid;

[0073] S12. The dried solid of S11 was ground and mixed with KOH at a mass ratio of 1:2.5, and then placed in a tube furnace for pyrolysis and carbonization under argon protection (heating rate of 10 °C / min to 900 °C, pyrolysis for 2.5 h), cooled to room temperature, washed with dilute hydrochloric acid and pure water several times until the solution was neutral, centrifuged to obtain a solid material, dried in an oven, and ground through a 200-mesh sieve to obtain biochar;

[0074] S13. The biochar after screening S12 was ground and mixed with urea in a mass ratio of 1:1.4, and then placed in a tubular furnace for pyrolysis and nitrogen doping under argon protection (heating rate of 5 °C / min to 370 °C, pyrolysis for 1.5 h), cooled to room temperature, washed with pure water several times until the solution was neutral, centrifuged to obtain a solid material, dried in an oven at 105 °C, and ground through a 200-mesh sieve to obtain a nitrogen-doped biochar carrier;

[0075] The specific surface area of ​​the nitrogen-doped biocarbon carrier is 2836.8 m 2 / g, and the nitrogen content is 3.7%.

[0076] A FeO x Nanocluster / nitrogen-doped biochar, the preparation process is as follows:

[0077] S1. Dissolve 0.06 g of phthalocyanine iron (II) in a mixed solution of 10 mL of ethanol and 10 mL of tetrahydrofuran, and stir until the phthalocyanine iron (II) is completely dissolved (about 10 min). At this time, the concentration of phthalocyanine iron (II) is 3 g / L; add 80 mg of the nitrogen-doped biocarbon carrier prepared above to the above phthalocyanine iron (II) solution. At this time, the volume ratio of the biocarbon carrier mass to the phthalocyanine iron (II) solution is 4.0 g: 1L, stir for 3 h, mix thoroughly, and evaporate to dryness at a constant temperature of 60°C with stirring to obtain a precursor;

[0078] S2. The precursor of S1 was placed in a tube furnace, heated to 900°C at a rate of 5°C / min in N2, pyrolyzed at 900°C for 1 h, cooled to room temperature, washed with water until neutral, dried, and ground to obtain FeO x Nanocluster / nitrogen-doped biochar, the theoretical iron content is about 6.9%.

[0079] Comparative Example 1

[0080] The specific preparation method of the biocarbon carrier in this comparative example is as follows:

[0081] S11. The washed and dried wheat bran biomass raw material is crushed and passed through a 0.3 mm sieve to obtain biomass powder, and the biomass powder is added to a certain volume of zinc chloride aqueous solution at a mass ratio of 1:1 to zinc chloride, wherein the concentration of zinc chloride in the zinc chloride aqueous solution is 200.0 g / L. After stirring for 20 minutes, the mixture is dried in an oven at 105°C, and the dried solid is placed in a tubular furnace for pyrolysis and carbonization under argon or nitrogen protection, i.e., the temperature is increased to 500°C at a rate of 10°C / min, and pyrolysis is performed for 1.0 h. After cooling to room temperature, the mixture is washed with dilute hydrochloric acid and pure water for several times until the solution is neutral, and the solid material is obtained by centrifugation, and dried in an oven at 105°C to obtain a solid.

[0082] S12: The dried solid of S11 was ground and mixed with KOH in a mass ratio of 1:2, and then placed in a tube furnace for pyrolysis and carbonization under argon or nitrogen protection (heating rate of 10 °C / min to 900 °C, pyrolysis for 2 h), cooled to room temperature, washed several times with dilute hydrochloric acid and pure water until the solution was neutral, centrifuged to obtain a solid material, dried in an oven, and ground through a 200-mesh sieve to obtain a biocarbon carrier. The specific surface area of ​​the obtained biocarbon carrier was 3200.8 m 2 / g.

[0083] A FeO x Nanoclusters / biochar, the preparation process is as follows:

[0084] S1. Dissolve 0.05 g of phthalocyanine iron (II) in a mixed solution of 10 mL of ethanol and 10 mL of tetrahydrofuran, and stir until the phthalocyanine iron (II) is completely dissolved (about 10 min). At this time, the concentration of phthalocyanine iron (II) is 2.5 g / L; add 100 mg of the above-prepared biocarbon carrier to the above phthalocyanine iron (II) solution. At this time, the ratio of the mass of the biocarbon carrier to the volume of the phthalocyanine iron (II) solution, i.e., the solid-liquid ratio, is 5.0 g / L. Stir for 3 h, mix thoroughly, and evaporate to dryness at a constant temperature of 60°C with stirring to obtain a precursor;

[0085] S2. The precursor of S1 was placed in a tube furnace, heated to 800℃ at a rate of 5℃ / min in an Ar atmosphere, and pyrolyzed at 800℃ for 2 h. After cooling to room temperature, it was washed with water until neutral, dried, and ground to obtain FeO x Nanocluster / nitrogen-doped biochar, the theoretical iron content is 4.7%.

[0086] The only difference between this comparative example and Example 1 is that the biochar carrier is not doped with nitrogen during the preparation process.

[0087] Comparative Example 2

[0088] The specific preparation method of the nitrogen-doped biocarbon carrier in this comparative example is consistent with that in Example 1; the specific surface area of ​​the nitrogen-doped biocarbon carrier is 2648.6 m 2 / g, and the nitrogen content is 3.5%.

[0089] A FeO x Nanocluster / nitrogen-doped biochar, the preparation process is as follows:

[0090] S1. Dissolve 0.1 g of phthalocyanine iron (II) in a mixed solution of 10 mL of ethanol and 10 mL of tetrahydrofuran, and stir until the phthalocyanine iron (II) is completely dissolved (about 10 min). At this time, the concentration of phthalocyanine iron (II) is 5 g / L; add 60 mg of the above-prepared biocarbon carrier to the above phthalocyanine iron (II) solution. At this time, the ratio of the mass of the biocarbon carrier to the volume of the phthalocyanine iron (II) solution, that is, the solid-liquid ratio, is 3 g / L. Stir for 3 h, mix thoroughly, and evaporate to dryness at a constant temperature of 60°C with stirring to obtain a precursor;

[0091] S2. The precursor of S1 was placed in a tube furnace, heated to 800°C at a rate of 5°C / min in an Ar atmosphere, pyrolyzed at 800°C for 2 h, cooled to room temperature, washed with water until neutral, dried, and ground to obtain FeO x Nanocluster / nitrogen-doped biochar, the theoretical iron content is 14.1%.

[0092] Effect Example 1

[0093] Experimental materials: FeO prepared in Example 1 x Nanocluster / nitrogen-doped biochar; FeO prepared in Comparative Example 1 x Nanoclusters / biochar.

[0094] Catalyst performance evaluation: mainly from two aspects: Fenton-like catalytic oxidation reaction and ozone peroxidation catalytic oxidation reaction;

[0095] Evaluation of Fenton-like catalytic oxidation effect:

[0096] Experimental method: The simulated pollutant is selected as 2,4,6-trichlorophenol, but not limited to 2,4,6-trichlorophenol. 100 mL of wastewater (the wastewater contains 2,4,6-trichlorophenol with a concentration of 56 mg / L) and 0.05 g of FeO x Nanoclusters / nitrogen-doped biochar or FeO x Nanoclusters / biochar were then added with 3.4 mL of 6% H2O2 solution to start the reaction. After 2 h of reaction, samples were taken and filtered using a 0.22 μm filter. The concentration of 2,4,6-trichlorophenol in the filtrate was immediately tested by HPLC.

[0097] Experimental results: The results show that the addition of FeO prepared in Example 1 x After using nanocluster / nitrogen-doped biochar as catalyst, the removal rate of 2,4,6-trichlorophenol reached 91.5%; while adding FeO prepared in Comparative Example 1 x After nanocluster / biochar was used as catalyst, the removal rate of 2,4,6-trichlorophenol was only 52.3%, which was lower than that of FeO prepared in Example 1. x The pollutant removal capacity of nanocluster / nitrogen-doped biochar was significantly decreased compared with that of biochar.

[0098] Evaluation of ozone peroxidation catalytic oxidation effect:

[0099] Experimental method: The simulated pollutant is selected from EDTA-Ni organic complex, but is not limited to EDTA-Ni organic complex. Add 100 mL of 5 mg / L Ni 2+ (Ni 2+ in the form of EDTA-Ni complex) and 0.05 g FeO xNanoclusters / nitrogen-doped biochar or FeOx nanoclusters / biochar, then 1.0 mL of 6% H2O2 solution was added, and ozone was introduced into the bottom of the reactor at the same time. The ozone concentration was 3.0 mg / L and the flow rate was 100 mL / min. The ozone that did not participate in the reaction at the reactor outlet was quenched with potassium iodide solution. The sample was taken after 45 min of reaction. The ozone in the sampled solution was first blown with N2, and then precipitated with DTC (dithiocarbamate) to remove the free Ni 2+ Then, the remaining undissociated Ni in the solution was determined by ICP (inductively coupled plasma). 2+ (EDTA-Ni organic complex not degraded by the reaction), with Ni in the EDTA-Ni organic complex 2+ to evaluate its removal effect.

[0100] Experimental results: The results show that the addition of FeO prepared in Example 1 x After the nanocluster / nitrogen-doped biochar was used as catalyst, Ni 2+ The concentration of the wastewater was lower than the detection limit, that is, the EDTA-Ni complex in the wastewater was effectively degraded after the reaction, reaching the emission standard (<0.1 mg / L) specified in the "Emission Standard of Electroplating Pollutants" (GB21900-2008); while the FeO prepared in Comparative Example 1 was added x After nanocluster / biochar was used as catalyst, Ni 2+ The concentration of FeO prepared in Example 1 is still 3.95 mg / L, which does not meet the emission standard (<0.1 mg / L) specified in the "Emission Standard of Electroplating Pollutants" (GB21900-2008). x The pollutant removal capacity of nanocluster / nitrogen-doped biochar was significantly decreased compared with that of biochar.

[0101] In the embodiment, biochar with high specific surface area and rich doping nitrogen content is selected as the carrier. Due to the large specific surface area and high doping nitrogen content of the carrier, a large number of anchoring points are provided for phthalocyanine iron (II), thereby inhibiting the agglomeration of phthalocyanine iron (II) during the pyrolysis process. After pyrolysis, FeO with high loading, extremely small particle size and high dispersion can be obtained. x Nanocluster catalytic active centers, while FeO x Nanoclusters / nitrogen-doped biochar also contain abundant Fe-N5 groups, which can promote the electron transfer of the catalyst. It can show excellent catalytic activity in the degradation of organic pollutants in water by catalyzing H2O2 alone (Fenton-like oxidation reaction) or catalyzing O3 / H2O2 (ozone peroxidation reaction).

[0102] In Comparative Example 1, the carrier is biochar without nitrogen doping, which fails to provide abundant N anchoring points. During the impregnation of iron phthalocyanine, iron phthalocyanine is randomly physically adsorbed (pore adsorbed) on the surface of the biochar carrier, which leads to the aggregation of iron ions and the formation of aggregated FeO after calcination. x Large particles, not highly active FeO x The nanoclusters, therefore, cannot effectively catalyze the reaction and thus exhibit low catalytic activity.

[0103] Effect Example 2

[0104] Experimental materials: FeO prepared in Example 2 x Nanocluster / nitrogen-doped biochar.

[0105] Catalyst performance evaluation: mainly from two aspects: Fenton-like catalytic oxidation reaction and ozone peroxidation catalytic oxidation reaction;

[0106] Evaluation of Fenton-like catalytic oxidation performance:

[0107] The simulated pollutant is selected from the antibiotic sulfamethoxazole, but is not limited to the antibiotic sulfamethoxazole. 100 mL of wastewater (the wastewater contains sulfamethoxazole at a concentration of 72 mg / L) and 0.05 g FeO x Nanocluster / nitrogen-doped biochar catalyst was added, and then 3.4 mL of 6% H2O2 solution was added to start the reaction. After 2 h of reaction, samples were taken and filtered through a 0.22 μm filter and immediately tested for concentration using HPLC. The results showed that the removal rate of sulfamethoxazole reached 92.3%.

[0108] Evaluation of ozone peroxidation catalytic oxidation performance:

[0109] The simulated pollutant is selected from EDTA-Ni organic complex, but is not limited to EDTA-Ni organic complex. 100 mL of 5 mg / L Ni 2+ (Ni 2+ Wastewater in the form of EDTA-Ni complex and 0.05FeO x Nanocluster / nitrogen-doped biochar catalyst, then add 1.0 mL of 6% H2O2 solution, and at the same time introduce ozone into the bottom of the reactor. The concentration of ozone is 3.0 mg / L and the flow rate is 100 mL / min. The ozone that does not participate in the reaction at the reactor outlet is quenched with potassium iodide solution. Samples are taken after 45 minutes of reaction. The ozone in the sampled solution is first blown with N2, and then precipitated with DTC to remove the free Ni 2+ , and then use ICP to determine the remaining undissociated Ni in the solution 2+(EDTA-Ni organic complex not degraded by the reaction), with Ni in the EDTA-Ni organic complex 2+ The results showed that the remaining undissociated Ni in the solution 2+ The concentration is 0.02 mg / L, which meets the emission standard (<0.1 mg / L) specified in the "Emission Standard of Pollutants from Electroplating" (GB21900-2008).

[0110] The FeO prepared in this example x The theoretical loading capacity of iron in nanocluster / nitrogen-doped biochar is as high as 3.3%, and it shows high catalytic activity in the degradation of organic pollutants in water by catalyzing H2O2 alone (Fenton-like oxidation reaction) or catalyzing O3 / H2O2 (ozone peroxidation reaction).

[0111] Effect Example 3

[0112] Experimental materials: FeO prepared in Example 3 x Nanocluster / nitrogen-doped biochar, FeO prepared in Comparative Example 2 x Nanocluster / nitrogen-doped biochar.

[0113] Catalyst performance evaluation: mainly from two aspects: Fenton-like catalytic oxidation reaction and ozone peroxidation catalytic oxidation reaction;

[0114] Evaluation of Fenton-like catalytic oxidation performance:

[0115] Experimental method: The simulated pollutant is selected from dye acid orange 7, but is not limited to dye acid orange 7. 100 mL of wastewater (the wastewater contains dye acid orange 7 with a concentration of 100 mg / L) and 0.05 g of FeO prepared in Example 3 are added to a cylindrical glass reaction container. x FeO prepared by nanocluster / nitrogen-doped biochar or comparative example 2 x The nanocluster / nitrogen-doped biochar was then added with 3.4 mL of 6% H2O2 solution to start the reaction. After 2 h of reaction, samples were taken and filtered using a 0.22 μm filter and immediately tested for its concentration using HPLC.

[0116] Experimental results: The results show that the addition of FeO prepared in Example 3 x After the nanocluster / nitrogen-doped biochar was used as a catalyst, the removal rate of dye acid orange 7 reached 90.8%. x When nanocluster / nitrogen-doped biochar was used as catalyst, the removal rate of dye acid orange 7 was only 61.5%, which was comparable to that of FeO prepared in Example 3. x The pollutant removal capacity of nanocluster / nitrogen-doped biochar was significantly decreased compared with that of biochar.

[0117] Evaluation of ozone peroxidation catalytic oxidation performance:

[0118] Experimental method: The simulated pollutant is selected from EDTA-Ni organic complex, but is not limited to EDTA-Ni organic complex. Add 100 mL of 5 mg / L Ni 2+ (Ni 2+ In the form of EDTA-Ni complex), 0.05 g of FeO prepared in Example 3 x FeO prepared by nanocluster / nitrogen-doped biochar or comparative example 2 x Nanocluster / nitrogen doped biochar, then added 1.0 mL of 6% H2O2 solution, and at the same time introduced ozone into the bottom of the reactor, the concentration of ozone was 3.0 mg / L, the flow rate was 100 mL / min, the ozone that did not participate in the reaction at the reactor outlet was quenched with potassium iodide solution, and the sample was taken after 45 min of reaction; the ozone in the sampled solution was first blown with N2, and then DTC was used for precipitation to remove the free Ni 2+ , and then use ICP to determine the remaining undissociated Ni in the solution 2+ (EDTA-Ni organic complex not degraded by the reaction), with Ni in the EDTA-Ni organic complex 2+ to evaluate its removal effect.

[0119] Experimental results: The results show that the addition of FeO prepared in Example 3 x ICP determination of the remaining Ni in the solution after using nanocluster / nitrogen-doped biochar as catalyst 2+ , its concentration is 0.08 mg / L; while adding FeO prepared in Comparative Example 2 x After nanocluster / nitrogen-doped biochar was used as catalyst, Ni 2+ The concentration of FeO prepared in Example 3 was still 3.23 mg / L, which did not meet the emission standard (<0.1 mg / L) specified in the "Emission Standard of Electroplating Pollutants" (GB21900-2008). x The pollutant removal capacity of nanocluster / nitrogen-doped biochar was significantly decreased compared with that of biochar.

[0120] The above catalytic effect difference is because, in Comparative Example 2, although a high specific surface area (2648.6 m 2 / g) of nitrogen-doped (3.5% N) biocarbon carrier, but due to the low solid-liquid ratio during the impregnation of iron phthalocyanine, a large amount of iron phthalocyanine still accumulated on the surface of the biocarbon carrier, and aggregated FeO was generated after calcination. x Large particles, not highly active FeO x The nanoclusters, therefore, cannot effectively catalyze the reaction and thus exhibit low catalytic activity.

[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. For ordinary technicians in this field, other different forms of changes or modifications can be made based on the above descriptions and ideas. It is not necessary and impossible to list all the implementation methods here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A kind of FeO x The method for preparing nanocluster / nitrogen-doped biochar is characterized in that: The following steps are involved: S1. placing the nitrogen-doped biocarbon carrier in an iron (II) phthalocyanine solution, immersing and evaporating at 40-60°C to obtain a precursor; S2. Take the precursor described in S1 and pyrolyze it at 700-900°C under an inert atmosphere, and then post-treat it to obtain FeO x Nanoclusters / nitrogen-doped biochar; The mass volume ratio of the nitrogen-doped biocarbon carrier to the phthalocyanine iron (II) solution is 4.0-5.8 g:1 L; the concentration of phthalocyanine iron (II) in the phthalocyanine iron (II) solution is 2.0-3.0 g / L; The specific surface area of ​​the nitrogen-doped biocarbon carrier is ≥ 2000 m 2 / g, and N content ≥3.0%; In the iron (II) phthalocyanine solution, the solvent is a mixed solution of ethanol and tetrahydrofuran in a volume ratio of 1: (0.8-1.2); The heating rate of the pyrolysis is 3-10°C / min; the pyrolysis time is 1-4 h.

2. The preparation method according to claim 1, characterized in that: The mass volume ratio of the nitrogen-doped biocarbon carrier to the iron phthalocyanine (II) solution is 4.5-5.5 g:1L.

3. The preparation method according to claim 1, characterized in that: The inert atmosphere is nitrogen or argon.

4. FeO prepared by any one of the preparation methods of claims 1 to 3 x Nanocluster / nitrogen-doped biochar.

5. FeO according to claim 4 x Application of nanocluster / nitrogen-doped biochar as hydrogen peroxide catalyst for degradation of organic pollutants in water.

6. FeO according to claim 4 x Application of nanocluster / nitrogen-doped biochar in catalytic O3 / H2O2 ozone peroxidation for degradation of organic pollutants in water.