A molecular sieve catalyst for preparing green aviation kerosene by one-step hydrogenation of biomass oil and its preparation method and application

By loading precious metals and non-precious metal additives on the ten-membered ring silicon aluminum molecular sieve and performing organic phosphorus repair, the problem of high stability and cost of molecular sieve in the hydrogenation reaction of bio-oil is solved, and the high activity and stability of the catalyst is achieved , suitable for making green aviation kerosene by one-step hydrogenation of bio-greases.

CN118698597BActive Publication Date: 2024-11-22SHANTOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411187407.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing ten-membered ring silicon aluminum molecular sieve is prone to damage to the skeleton structure due to adsorption and attack of water molecules, deactivation of the catalyst, and weak acidity, high process cost and poor stability.

Method used

The precious metal and non-precious metal additives are loaded on the ten-membered ring silicon aluminum molecular sieve repaired by organophosphorus. Si-OH is activated by fluoride and small-molecular organophosphorus is coupled to reduce uncoordinated saturation sites, inhibit water molecules adsorption, and improve catalysts. Activity and stability.

Benefits of technology

It significantly improves the activity, selectivity and stability of the catalyst, reduces operating costs, has a wide range of adaptation and high reproducibility, and is suitable for high oxygen-containing compound reaction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118698597B_ABST
    Figure CN118698597B_ABST
Patent Text Reader

Abstract

The present invention relates to a biomass oil one-step hydrogenation green aviation kerosene molecular sieve catalyst, including a ten-membered ring silicon aluminum molecular sieve repaired by precious organic phosphorus and a precious metal and a non-precious metal auxiliary agent loaded on the ten-membered ring silicon aluminum molecular sieve repaired by organic phosphorus; the precious metal and the non-precious metal auxiliary agent account for 0.2% to 3% and 10% to 30% by weight of the element respectively. The ten-membered ring silicon aluminum molecular sieve repaired by organic phosphorus is first activated by fluoride and then coupled with small molecule organic phosphorus to obtain; the biomass oil includes soybean oil, palm oil, olive oil, peanut oil, jatropha oil, rapeseed oil, cottonseed oil, castor oil, tung oil and waste grease; the precious metal is one of Pt, Pd and Ru, and the non-precious metal is one of Ni, Co, Ce, La and Fe. The catalyst of the present invention has high stability and catalytic activity, can be used for one-step hydrogenation of biomass oil to produce green aviation kerosene, mild reaction conditions, high conversion rate, high isomeric hydrocarbon ratio, good stability, and high tolerance to oxygen-containing compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a molecular sieve catalyst for preparing green aviation kerosene by one-step hydrogenation of biomass oil, and a preparation method and application thereof. Background Art

[0002] SAF, also known as green aviation fuel, produces 60-80% less carbon dioxide than traditional aviation fuel and is the only solution that can reduce the carbon emission intensity of air travel in the near future. Among the many green aviation fuel production routes, the hydrotreated ester and fatty acid kerosene route (HEFA) is to obtain bio-jet fuel by hydrorefining and hydroisomerization of bio-oils such as vegetable oils and waste oils. Compared with other technical routes, the HEFA route has the advantages of high technical maturity, simple process flow, and wide application range. It is the most promising technical route to meet the demand for green aviation fuel in the short term. Since the main component of bio-oil is higher fatty acid triglyceride, it has a large relative molecular mass, high unsaturated hydrocarbon content and high oxygen content, so it needs to be hydrodeoxygenated to reduce the oxygen content and obtain normal alkanes; then, the obtained long-chain alkanes need to be hydroisomerized to reduce the freezing point of the oil and improve the low-temperature flow performance to obtain high-quality green aviation fuel.

[0003] It can be seen that the hydrodeoxygenation and hydroisomerization processes of the process of producing high-quality green aviation kerosene using bio-oil as raw materials through hydrogenation technology require multiple reactors, multi-step operations and multiple catalysts. The equipment occupies a large area and has high operating and maintenance costs, and the economic benefits are poor. The one-step hydrogenation of bio-oil to produce green aviation kerosene refers to the reaction raw materials completing a series of hydrogenation reactions (hydrodeoxygenation and hydroisomerization) in a single reactor. It has the advantages of short reaction route, low energy consumption and low operating cost, and has become the focus of researchers.

[0004] The catalyst for one-step hydrogenation of biomass oil to produce green aviation kerosene is a bifunctional catalyst composed of a metal component and an acidic component, in which the metal component plays the role of hydrodeoxygenation and hydrodehydrogenation, and Pt, Pd, Ni, Mo, Co and other metals are mostly used. The acidic carrier plays the role of protonation and hydrocarbon skeleton rearrangement, and one-dimensional ten-membered ring silicon aluminum ZSM-23, ZSM-22, ZSM-48 molecular sieves and aluminum phosphate SAPO-11 molecular sieves are mostly used. However, the oxygen content in bio-oil is relatively high, and water is generated during the hydrogenation and removal process, which can easily cause the migration of Si and Al species in the framework of the silicon aluminum molecular sieve during the high temperature and high pressure reaction process, and deposit in the molecular sieve pores, causing the framework to collapse and the catalyst to be irreversibly deactivated.

[0005] In order to solve the stability problem of molecular sieve catalysts in the hydrogenation process of bio-oils, researchers can only use aluminum phosphate SAPO-11 molecular sieve. However, the high cost of the synthesis process and low mechanical strength of SAPO-11 molecular sieve are difficult to solve, and due to its weak acidity, the hydrogenation isomerization reaction needs to be carried out at a higher temperature (>350 ℃), which leads to increased side reactions and high operating costs. Therefore, it is a better choice to use ZSM-23, ZSM-22, ZSM-48, and ZSM-35 with low synthesis cost, high reaction activity, good mechanical strength, and strong acidity. However, the Si-OH species widely present in silicon-aluminum ZSM-23, ZSM-22, ZSM-48, and ZSM-35 molecular sieves are the main adsorption and attack sites of water molecules, which not only affects the physical and chemical properties of the molecular sieve such as crystallinity and acidity, but also causes the molecular sieve to have poor stability in a reaction environment containing water or water generation. Summary of the invention

[0006] The purpose of the present invention is to provide a biomass oil one-step hydrogenation to green aviation kerosene molecular sieve catalyst and its preparation method and application, to solve the existing problem that when the one-dimensional ten-membered ring silicon aluminum molecular sieve is used for the one-step hydrogenation reaction of bio-oil, the uncoordinated saturated silicon and aluminum species in the one-dimensional ten-membered ring silicon aluminum molecular sieve framework are the main adsorption and attack sites of water generated by hydrogenation and deoxygenation, which is easy to cause the destruction of the molecular sieve framework structure, irreversible deactivation of the catalyst, etc., resulting in low catalyst activity, product yield and poor hydrothermal stability. The molecular sieve catalyst prepared by the present invention has excellent activity, selectivity and stability in the route of one-step hydrogenation of bio-oil to green aviation kerosene, and the molecular sieve control scheme is highly operable, has a wide range of adaptability and high reproducibility.

[0007] A biomass oil one-step hydrogenation to green aviation kerosene molecular sieve catalyst, comprising a precious metal, a non-precious metal additive and an organophosphorus repaired ten-membered ring silica-alumina molecular sieve; the precious metal and the non-precious metal additive are loaded on the organophosphorus repaired ten-membered ring silica-alumina molecular sieve; the precious metal in the catalyst accounts for 0.2% to 3% by mass as an element, and the non-precious metal additive accounts for 10% to 30% by mass as an element.

[0008] The role of non-precious metals is to assist the hydrogenation activity of precious metals, while enhancing the dispersion of precious metal sites and, to a certain extent, controlling the distance between metal sites and acid sites, thereby reducing the occurrence of cracking side reactions in the hydrogenation isomerization reaction.

[0009] Furthermore, the organophosphorus repaired ten-membered ring silicon-aluminum molecular sieve is obtained by first activating Si-OH in the ten-membered ring silicon-aluminum molecular sieve with fluoride, and then coupling small molecule organophosphorus; the ten-membered ring silicon-aluminum molecular sieve includes at least one of ZSM-23, ZSM-48, ZSM-22, ZSM-35, and EU-1. The one-dimensional ten-membered ring channel silicon-aluminum molecular sieve can be a sodium type, potassium type, hydrogen type, or ammonia type molecular sieve powder. More preferably, the silicon-aluminum molar ratio of the molecular sieve powder is 25 to 1000.

[0010] The present invention first uses fluoride to activate Si-OH in the silicon-alumina molecular sieve and couples small molecule organic phosphorus. On the one hand, Si-OH species are converted into Si-O-Si to reduce the uncoordinated saturated skeleton structure. On the other hand, P species are modified in the molecular sieve structure to further inhibit the adsorption of water molecules on the molecular sieve skeleton, thereby improving the activity of the catalyst and the product yield, and achieving a significant improvement in stability.

[0011] Furthermore, the biomass oil is animal or plant oil, including one or more of soybean oil, palm oil, olive oil, peanut oil, jatropha oil, rapeseed oil, cottonseed oil, castor oil, tung oil, and waste oil.

[0012] Furthermore, the noble metal is one of Pt, Pd, and Ru, and the non-noble metal is one of Ni, Co, Ce, La, and Fe.

[0013] The biomass oil can be a fatty acid model compound selected from alcohols, acids, aldehydes, ketones with different carbon numbers, preferably alcohols, acids, aldehydes, ketones with oxygen-containing functional groups located at the ends of the carbon chains.

[0014] The proportion of saturated fatty acids in biomass oil is 20~50 wt%, the proportion of monounsaturated fatty acids is 10~30 wt%, and the proportion of polyunsaturated fatty acids is 40~60 wt%.

[0015] The method for preparing the molecular sieve catalyst for preparing green aviation kerosene by one-step hydrogenation of biomass oil comprises the following steps:

[0016] (1) uniformly mixing an extrusion aid, a binder and an organophosphorus-repaired ten-membered ring silicon-aluminum molecular sieve;

[0017] (2) Add the peptizing agent and mix into a paste, stir for 0.5-2 h, and then place in a mold for extrusion molding;

[0018] (3) Then, the sample obtained in step (2) is placed in an oven at 80-180°C and dried for 10-24 hours;

[0019] (4) Collect the product of step (3) and calcine it at 300-600°C for 3-60 h. The solid product can be collected by vacuum filtration and centrifugal separation.

[0020] (5) dripping a solution containing a noble metal salt onto the calcined product obtained in step (4), drying it at room temperature for 1-3 h, then drying it at a drying temperature of 110 °C for 12 h, and then calcining it at a temperature of 550 °C for 6 h to obtain a single metal supported catalyst;

[0021] (6) Then, the non-precious metal salt solution is dropped into the monometallic supported catalyst obtained in step (5), and the catalyst is dried at room temperature for 1-3 h, then dried at 110 °C for 12 h, and then calcined at 550 °C for 6 h.

[0022] The extrusion aid in step (1) includes at least one of sesbania powder, methyl cellulose, starch, polyvinyl alcohol and polyethanol; the binder includes one or more of pseudo-boehmite, acidic silica sol, alkaline silica sol and kaolin.

[0023] The peptizing agent in step (2) is an organic acid and / or an inorganic acid.

[0024] The main functions of the molecular sieve forming process in step (2) are: processing the molecular sieve into a certain shape to meet the filling requirements of different types of reactors; making the molecular sieve finished product have a certain strength to ensure that the molecular sieve finished product resists the damage to its structure caused by process conditions (such as temperature, pressure, fluid scouring, regeneration, etc.) during use. The higher the strength of the molecular sieve finished product, the less powdering during use, the smaller the pressure drop of the bed, and the longer the service life. The molecular sieve forming process can be formed by rolling ball method, tableting method and extrusion method. The shape after forming can be clover-shaped, butterfly-shaped, cylindrical, hollow cylindrical, four-leaf, five-leaf or spherical, etc.

[0025] Furthermore, the mass ratio of the organic phosphorus repaired ten-membered ring silica-alumina molecular sieve, extrusion aid, peptizing agent and adhesive is 1: 0.1~5: 0.1~1.5: 0.3~2.

[0026] The precious metal precursor is selected from chloroplatinic acid, platinum chloride, tetraammonium platinum nitrate, tetraammonium platinum dichloride, platinum nitrate, palladium nitrate, palladium chloride, palladium acetate, sodium tetrachloropalladate, dichlorotetraamminepalladium, ruthenium chloride, ruthenium nitrate, ruthenium acetylacetonate, ruthenium acetate, and ammonium hexachlororuthenate; the non-precious metal precursor is selected from cobalt nitrate, cobalt acetate, basic cobalt carbonate, cobalt chloride, nickel nitrate, nickel acetate, basic nickel carbonate, nickel chloride, and nickel carbonate.

[0027] The application of the above-mentioned biomass oil one-step hydrogenation to produce green aviation kerosene molecular sieve catalyst is used for the one-step hydrogenation of biomass oil.

[0028] The method for one-step hydrogenation of biomass oil to produce green aviation kerosene by using the molecular sieve catalyst is as follows: using biomass oil as raw material, reacting at a reaction temperature of 260-340 °C, a hydrogen-to-oil ratio of 50-4000:1, and a liquid hourly space velocity of 0.15-6 h -1 Under the condition of a pressure of 3.5-9 Mpa, the biomass oil one-step hydrogenation to produce green aviation kerosene molecular sieve catalyst is placed in a fixed bed reactor to carry out a one-step hydrogenation reaction of the biomass oil.

[0029] A method for preparing an organophosphorus-repaired ten-membered ring silicon-aluminum molecular sieve comprises the following steps:

[0030] (S1) preparing a mixed solution with an organophosphorus, a fluoride and deionized water in a mass ratio of 1:0.6-2.5:2-45;

[0031] (S2) adding one-dimensional ten-membered ring silica-alumina molecular sieve powder to the mixed solution prepared in step (S1) in a stirring state in a mass ratio of 1:5-90 to the total mass of the one-dimensional mesoporous silica-alumina molecular sieve, stirring for 1-10 hours at a temperature of 30-95° C., and transferring to a reaction kettle after being fully mixed; performing hydrothermal treatment under certain conditions, wherein the treatment process is intended to further promote the interaction between the molecular sieve and other components in the solution through thermal effect;

[0032] (S3) Collecting the solid product obtained in step (S2), drying it at 80-130°C for 6-48 hours, and then transferring it to a muffle furnace and calcining it at a high temperature of 400-700°C for 3-8 hours.

[0033] The fluoride is selected from at least one of tetrapropylammonium fluoride, calcium fluoride, sodium fluoride, tetramethylammonium fluoride, hydrogen fluoride, tetrabutylammonium fluoride and tetraethylammonium fluoride. The organic phosphide is selected from at least one of tetramethylphosphonium bromide, tetraethylphosphonium bromide, tetrabutylphosphonium bromide, tetrabutylphosphonium hydroxide, tri-n-butylphosphine oxide and tetraphenylphosphonium bromide.

[0034] The organic phosphorus repaired ten-membered ring silicon-aluminum molecular sieve obtained by the above preparation method.

[0035] When cottonseed oil or waste oil is used as the raw material for performance testing, since the main components of the raw material are fatty acids and contain more oxygenated compounds, the products of its hydrogenation reaction contain not only normal alkanes and isoalkanes, but also cycloalkanes and aromatic hydrocarbons.

[0036] The molecular sieve catalyst prepared by the present invention is mainly used in the field of preparing green aviation kerosene by hydrogenation reaction of biomass oil. Biomass oil refers to animal and plant oils and fats, and its main component is higher fatty acid triglyceride, which has a large relative molecular mass, and a high content of unsaturated hydrocarbons and oxygen. The raw materials used in the performance test of the present invention are cottonseed oil and waste oil (gutter oil, catering waste oil) in daily life.

[0037] The main components of cottonseed oil are various fatty acids, among which palmitic acid, stearic acid, oleic acid and linoleic acid are more significant. In addition to various fatty acids, waste oil (gutter oil, restaurant waste oil) also contains a certain amount of water and solid impurities, and has a high content of oxygenated compounds. These two raw materials have complex compositions, many impurities and oxygenated compounds.

[0038] The molecular sieve catalyst prepared by the present invention has excellent activity, selectivity and stability in the route of one-step hydrogenation of bio-oil to produce green aviation kerosene, and the molecular sieve control scheme has strong operability, wide adaptability and high reproducibility.

[0039] The present invention adopts post-treatment technology to repair the existing molecular sieve framework structure, reduce uncoordinated saturated sites, and improve the crystallinity of the molecular sieve. The prepared hydrogenation catalyst shows high activity and isomer yield in the hydrogenation reaction of model compounds and real oil products; and due to the introduction of P species, it is difficult for the molecular sieve to undergo skeleton dealumination under the condition of water vapor, thereby achieving the goal of improving the hydrothermal stability of the molecular sieve. In addition, since the hydroxyl groups on the phosphorus atoms can provide proton acids, the repaired zeolite molecular sieve maintains a certain acid density, which is conducive to the obtained catalyst to show excellent catalytic stability and catalytic activity under reaction conditions with a high content of oxygen-containing compounds. The molecular sieve repair method provided by the present invention has strong operability, high reproducibility, and low cost. The catalyst of the present invention is applied to the hydrogenation reaction of bio-oils under mild conditions, high conversion rate, high ratio of isomerized hydrocarbons, good stability, and high tolerance to oxygen-containing compounds.

[0040] Compared with the prior art, the present invention repairs Si-OH into a saturated Si-O-Si four-coordinate structure, while introducing a PO bond into the structure of the molecular sieve, where P exists in a four-coordinate form. This interface structure makes it difficult for the molecular sieve to undergo skeleton dealumination under water vapor conditions, thereby improving the stability of the molecular sieve. Furthermore, because the hydroxyl group on the phosphorus atom can provide proton acid, the molecular sieve catalyst obtained after the repair by the present invention has both high stability and high catalytic activity, and can directly use vegetable oil or waste oil in real life as a reactant for the hydrogenation reaction catalyst performance test. The catalyst performance test conditions of the present invention are more stringent, and waste oil or vegetable oil does not need to be dehydrated, decolorized or de-impurified, and can be used directly as a reactant. The molecular sieve repair method provided by the present invention has strong operability, high reproducibility and low cost. The catalyst of the present invention is used in the hydrogenation reaction of bio-oil under mild reaction conditions, with high conversion rate, high isohydrocarbon ratio and good stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is the XRD spectra of Examples 1-9 and Comparative Examples 1-3;

[0042] Figure 2 29Si MAS NMR spectra of Example 3 and Comparative Example 1;

[0043] Figure 3 is the infrared spectra of Examples 1 to 6 and ZSM-48 molecular sieve raw powder;

[0044] Figure 4 The palmitic acid hydrogenation conversion performance comparison between the catalysts of Example 5 and Comparative Example 1 at different temperatures;

[0045] Figure 5 The stability test results of the catalyst obtained in Example 5 when cottonseed oil is used as the raw material;

[0046] Figure 6 This is the stability test result of the catalyst obtained in Example 5 when waste oil is used as raw material. DETAILED DESCRIPTION

[0047] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.

[0048] Example 1

[0049] A method for preparing a bio-oil one-step hydrogenation molecular sieve comprises the following steps:

[0050] (1) Add 120 g of a prepared mixed solution of tetraethylphosphine bromide and tetrabutylammonium fluoride at one time and mix with 10 g of ZSM-48 molecular sieve (silicon-aluminum ratio of 200), wherein the prepared mixed solution contains 14 g of tetraethylphosphine bromide, 65 g of tetrabutylammonium fluoride, and the remaining 41 g is water.

[0051] (2) The obtained suspension solution was stirred at 60 °C and 200 r / min for 6 h, then transferred to a high-pressure reactor and statically reacted at 160 °C for 12 h, followed by vacuum filtration, and the solid was fully washed with deionized water. The obtained solid product was placed in an oven for drying to remove moisture. The drying temperature was 80 °C and the drying time was 12 h. The dried product was then placed in a muffle furnace for calcination at 600 °C and the calcination time was 6 h to obtain a highly stable ZSM-48 molecular sieve, which was labeled as L1. The XRD spectrum and infrared spectrum of the L1 sample are shown as follows: Figure 1 and Figure 3 The crystallinity of the prepared samples calculated from the XRD data is shown in Table 1.

[0052] (3) Take 6 g of sesbania powder, 3 g of pseudo-boehmite and 4 g of L1 molecular sieve obtained above and mix them evenly. Then add 14 g of citric acid to make a paste. After stirring for 0.5 h, put it into a mold for extrusion molding. Then, the obtained sample is placed in an oven at 80 °C for 12 h and then calcined in a muffle furnace at 600 °C for 6 h to obtain a shaped solid acid carrier.

[0053] (4) Using the immersion method, a solution containing 3.67 g of palladium nitrate metal salt was slowly dripped into the formed solid acid carrier, dried at room temperature for 2 h, and then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at 550 °C for 6 h to obtain a single metal supported catalyst.

[0054] (5) Using an immersion method, a solution containing 5.62 g of nickel nitrate metal salt was slowly dripped into the catalyst precursor described in step (4), and then dried at room temperature for 2 h. It was then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at a temperature of 550 °C for 6 h to finally obtain a bimetallic supported catalyst, which was labeled as Z1.

[0055] Example 2

[0056] The catalyst was prepared by referring to the method described in Example 1, except that the reaction kettle was subjected to dynamic reaction at 160°C for 12 h and the rotation speed was 70 rpm. The prepared molecular sieve was marked as L2, and the obtained metal-supported catalyst was marked as Z2. The XRD spectrum and infrared spectrum of L2 are shown in Figures 1 and 2, respectively. Figure 1 and Figure 3 The crystallinity of the samples calculated from the XRD data is shown in Table 1.

[0057] Example 3

[0058] A method for preparing a highly stable molecular sieve comprises the following steps:

[0059] (1) Add 120 g of the prepared mixed solution of tri-n-butylphosphine oxide and calcium fluoride in stages and mix it with 10 g of ZSM-48 molecular sieve (silicon-aluminum ratio of 200) for multiple times, wherein 40 g of tri-n-butylphosphine oxide and 12 g of calcium fluoride are added to the prepared mixed solution.

[0060] (2) Take 40 g of a mixed solution of tri-n-butylphosphine oxide and calcium fluoride and add it to 10 g of ZSM-48 molecular sieve, stir it at 60 °C and 200 r / min for 2 h, then add another 40 g of a mixed solution of tri-n-butylphosphine oxide and calcium fluoride and continue stirring for 2 h. Finally, add the remaining mixed solution and continue stirring for 2 h. Then transfer it to a high-pressure reactor and react it dynamically at 160 °C for 12 h. The speed is set to 70 rpm. Then vacuum filter it and wash the solid with deionized water. The washed solid product is placed in an oven for drying to remove moisture. The drying temperature is 80 °C and the drying time is 12 h. Then the dried product is placed in a muffle furnace for calcination at 600 °C and the calcination time is 6 h. A highly stable ZSM-48 molecular sieve is obtained and is labeled as L3. The XRD spectrum and infrared spectrum of the L3 sample are shown as follows: Figure 1 and Figure 3 The crystallinity of the prepared sample calculated from the XRD data is shown in Table 1, and the prepared L3 was subjected to solid nuclear magnetic resonance testing, and the results are shown in Figure 2 shown.

[0061] (3) Take 6 g of methyl cellulose, 3 g of pseudo-boehmite and 4 g of the L3 molecular sieve obtained above and mix them evenly. Then, add 14 g of dilute nitric acid to make a paste. After stirring for 0.5 h, the paste is placed in a mold for extrusion molding. The obtained sample is then placed in an oven at 80 °C for 12 h and then calcined in a muffle furnace at 600 °C for 6 h to obtain a molded solid acid carrier.

[0062] (4) Using the immersion method, a solution containing 3.21 g of chloroplatinic acid metal salt was slowly dripped into the formed solid acid carrier, dried at room temperature for 2 h, and then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at 550 °C for 6 h to obtain a single metal supported catalyst.

[0063] (5) Using the immersion method, a solution containing 5.81 g of cobalt nitrate metal salt was slowly dripped into the catalyst precursor described in step (4), and then dried at room temperature for 2 h. It was then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at a temperature of 550 °C for 6 h to finally obtain a bimetallic supported catalyst, which was labeled as Z3.

[0064] Example 4

[0065] A method for preparing a highly stable molecular sieve comprises the following steps:

[0066] (1) Add 120 g of the prepared mixed solution of tetraphenylphosphonium bromide and tetramethylammonium fluoride in stages and mix it with 10 g of ZSM-48 molecular sieve (silicon-aluminum ratio of 200) for multiple times, wherein 39 g of tetraphenylphosphonium bromide and 14 g of tetramethylammonium fluoride are added to the prepared mixed solution.

[0067] (2) Take 40 g of the mixed solution of tetraphenylphosphonium bromide and tetramethylammonium fluoride and add it to 10 g of ZSM-48 molecular sieve, place it at room temperature and stir it at 200 r / min for 2 h, then add 40 g of the mixed solution of tetraphenylphosphonium bromide and tetramethylammonium fluoride, place it at 50 °C and 200 r / min and continue to stir it for 2 h, finally add the remaining mixed solution, place it at 90 °C and 200 r / min and continue to stir it for 2 h, then transfer it to a high-pressure reactor and dynamically react it at 160 °C for 12 h with the speed set to 70 rpm, then vacuum filter it, wash the solid thoroughly with deionized water, dry it in an oven after washing to remove moisture, the drying temperature is 80 °C, the drying time is 12 h, then place the dried product in a muffle furnace for calcination at 600 °C for 6 h to obtain a highly stable ZSM-48 molecular sieve, which is labeled as L4. The XRD spectrum and infrared spectrum of L4 sample are shown in Figure 1 and Figure 3 The crystallinity of the prepared samples calculated from the XRD data is shown in Table 1.

[0068] (3) Take 6 g of starch, 3 g of alkaline silicon solution and 4 g of L4 molecular sieve obtained above and mix them evenly, then add 14 g of tartaric acid to make a paste. After stirring for 0.5 h, put it into a mold for extrusion molding, and then place the obtained sample in an oven at 80 °C for 12 h, and then place it in a muffle furnace for calcination at 600 °C for 6 h to obtain a molded solid acid carrier.

[0069] (4) Using the immersion method, a solution containing 3.41 g of tetraammonium nitrate platinum salt was slowly dripped into the formed solid acid carrier, dried at room temperature for 24 h, and then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at 550 °C for 6 h to obtain a single metal supported catalyst.

[0070] (5) Using an immersion method, a solution containing 4.27 g of nickel nitrate metal salt was slowly dripped into the catalyst precursor described in step (4), and the mixture was dried at room temperature for 24 h. The mixture was then placed in an oven for drying at a temperature of 110 °C for 12 h. The mixture was then calcined in a muffle furnace at a temperature of 550 °C for 6 h to obtain a bimetallic supported catalyst, which was labeled as Z4.

[0071] Example 5

[0072] The catalyst was prepared by referring to the method described in Example 4, except that the high-pressure reactor was subjected to dynamic reaction at 160°C for 12 h and the rotation speed was 20 rpm. The prepared molecular sieve was labeled as L5, and the obtained bimetallic supported catalyst was labeled as Z5. The XRD spectrum and infrared spectrum of L5 are shown in Figures 1 and 2, respectively. Figure 1 and Figure 3 The crystallinity of the samples calculated from the XRD data is shown in Table 1.

[0073] Example 6

[0074] The catalyst was prepared by referring to the method described in Example 4, except that the prepared mixed solution was added into 10 g of ZSM-48 molecular sieve reactor at one time for mixing, the prepared molecular sieve was marked as L6, and the obtained bimetallic supported catalyst was marked as Z6. The XRD spectrum and infrared spectrum of L6 are shown in Figure 1 and Figure 3 The crystallinity of the samples calculated from the XRD data is shown in Table 1.

[0075] Example 7

[0076] The catalyst was prepared by referring to the method described in Example 5, except that the ZSM-48 molecular sieve was replaced with a ZSM-23 molecular sieve (silicon-aluminum ratio of 250), the prepared molecular sieve was marked as L7, and the obtained bimetallic supported catalyst was marked as Z7. The XRD spectrum of L7 is shown in Figure 1 The crystallinity of the samples calculated from the XRD data is shown in Table 1.

[0077] Example 8

[0078] The catalyst was prepared by referring to the method described in Example 7, except that 26 g of sodium fluoride was used to replace tetramethylammonium fluoride in Example 7, the prepared molecular sieve was marked as L8, and the obtained bimetallic supported catalyst was marked as Z8. The XRD spectrum of L8 is shown in Figure 1 The crystallinity of the samples calculated from the XRD data is shown in Table 1.

[0079] Example 9

[0080] The catalyst was prepared by referring to the method described in Example 7, except that 36 g of tetrabutylphosphonium bromide was used to replace tetraphenylphosphonium bromide in Example 7, the prepared molecular sieve was marked as L9, and the obtained bimetallic supported catalyst was marked as Z9. The XRD spectrum of L9 is shown in Figure 1 The crystallinity of the samples calculated from the XRD data is shown in Table 1.

[0081] Comparative Example 1

[0082] A method for preparing a catalyst comprises the following steps:

[0083] (1) Take 6 g of sesbania powder, 3 g of kaolin and 4 g of ZSM-48 molecular sieve (silicon-aluminum ratio is 200) and mix them evenly. Then add 14 g of tartaric acid and mix them into a paste. After stirring for 0.5 h, place it in a mold for extrusion molding. Then, place the obtained sample in an oven at 80 °C for 12 h, and then place it in a muffle furnace for calcination at 600 °C for 6 h to obtain a molded solid acid carrier, which is marked as LD10. The ZSM-48 molecular sieve was tested by solid nuclear magnetic resonance. The results are as follows: Figure 2 shown.

[0084] (2) Using the immersion method, a solution containing 3.32 g of tetraammonium nitrate platinum salt was slowly dripped into the formed solid acid carrier, dried at room temperature for 2 h, and then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at 550 °C for 6 h to obtain a single metal supported catalyst.

[0085] (3) Using an immersion method, a solution containing 4.23 g of nickel nitrate metal salt was slowly dripped into the catalyst precursor described in step (2), and the mixture was dried at room temperature for 2 h. The mixture was then placed in an oven for drying at a temperature of 110 °C for 12 h. The mixture was then calcined in a muffle furnace at a temperature of 550 °C for 6 h to obtain a bimetallic supported catalyst, which was labeled as ZD10.

[0086] Comparative Example 2

[0087] A method for preparing a catalyst comprises the following steps:

[0088] (1) Add 120 g of the prepared ammonium fluoride solution into 10 g of ZSM-48 molecular sieve at one time and mix them. The amount of ammonium fluoride added to the prepared ammonium fluoride solution is 10 g.

[0089] (2) The suspension obtained in step (1) was stirred at 60 °C and 200 r / min for 2 h, and then transferred to a 160 °C autoclave for dynamic reaction at a speed of 20 rpm for 12 h. After that, vacuum filtration was performed, and the obtained solid was thoroughly washed with deionized water. Then, it was placed in an oven at 80 °C for drying to remove moisture. The drying time was 12 h. Finally, the dried solid product was placed in a muffle furnace and calcined at 600 °C for 6 h. It was labeled as LD11.

[0090] (3) Take 6 g of sesbania powder, 3 g of alkaline silicon solution and 4 g of LD11 molecular sieve obtained above and mix them evenly, then add 14 g of tartaric acid to make a paste. After stirring for 0.5 h, place it in a mold for extrusion molding, and then place the obtained sample in an oven at 80 °C for 12 h, and then place it in a muffle furnace for calcination at 600 °C for 6 h to obtain a molded solid acid carrier.

[0091] (4) Using the immersion method, a solution containing 2.31 g of chloroplatinic acid metal salt was slowly dripped into the formed solid acid carrier, dried at room temperature for 2 h, and then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at 550 °C for 6 h to obtain a single metal supported catalyst.

[0092] (5) Using the immersion method, a solution containing 6.31 g of cobalt nitrate metal salt was slowly dripped into the catalyst precursor described in step (4), and then dried at room temperature for 2 h. It was then placed in an oven for drying at a temperature of 110 °C for 12 h. It was then placed in a muffle furnace and calcined at a temperature of 550 °C for 6 h to finally obtain a bimetallic supported catalyst, which was labeled as ZD11.

[0093] Comparative Example 3

[0094] The catalyst was prepared by referring to the method described in Comparative Example 2, except that 120 g of a solution containing 28 g of tetraethylphosphine bromide was used to replace the ammonium fluoride solution in Comparative Example 2, the prepared molecular sieve was labeled LD12, and the obtained metal-supported catalyst was labeled ZD12. The XRD spectrum of LD12 is shown in FIG. Figure 1 The crystallinity of the samples calculated from the XRD data is shown in Table 1.

[0095] Performance Testing

[0096] 1. Catalytic reaction performance test

[0097] Using model compounds palmitic acid, cottonseed oil and waste oil as raw materials, respectively, at a reaction temperature of 260-340 ° C, a hydrogen-to-oil ratio of 1200: 1, a volume space velocity of 5 h-1, and a pressure of 4 MPa, 3 mL of the catalyst was placed in a fixed bed reactor, and the metal-supported molecular sieve catalyst prepared in the above-obtained examples and comparative examples was subjected to a one-step hydrogenation reaction of biomass oil. The performance test results are shown in Tables 2, 3 and Figure 4 .

[0098] Table 1 Crystallinity of all molecular sieve samples in various embodiments and comparative examples

[0099]

[0100] Table 2 The catalytic reaction performance results of the catalysts of each embodiment and each comparative example using palmitic acid as raw material

[0101]

[0102] 2. Stability performance test

[0103] Cottonseed oil and waste oil were used as raw materials, respectively, at a reaction temperature of 310 °C, a hydrogen-to-oil ratio of 1500:1, and a volume space velocity of 5.5 h -1 , under the condition of 4 MPa, 3 mL of the catalyst Z5 described in Example 5 was taken and placed in a fixed bed reactor to carry out a catalyst stability performance test. The test time was 1000 h. The catalyst stability performance test results were shown in Figure 5 and Figure 6 .

[0104] The present invention believes that in the process of enhancing the stability of molecular sieves, the uncoordinated saturated Si-OH groups on the crystal boundary of the silicon-aluminum molecular sieve are activated by fluoride, and some Si-OH species migrate out of the skeleton structure, condense with adjacent Si-OH groups, and dehydrate to form a saturated four-coordinated Si-O-Si structure; in this process, the P species mainly reacts with the terminal hydroxyl of Al in the molecular sieve to stabilize the skeleton, and after high-temperature roasting, a PO bond is formed, so that P exists in a four-coordinated form. This interface structure makes it difficult for the molecular sieve to dealuminate the skeleton under the condition of water vapor, thereby significantly improving the stability of the molecular sieve. In addition, since the hydroxyl on the phosphorus atom can provide proton acid, the treated molecular sieve has a certain acid density. Therefore, the catalyst prepared by the molecular sieve treated by the method of the present invention exhibits excellent catalytic stability and catalytic activity under reaction conditions with a high content of oxygen-containing compounds.

[0105] Figure 1 is the XRD spectra of the above-mentioned embodiments 1 to 9 and the comparative example, Figure 1 It can be seen that the repaired ZSM-48 molecular sieve and ZSM-23 molecular sieve both present typical characteristic diffraction peaks of MRE and MTT, respectively. No obvious shift is observed in the position of the characteristic diffraction peaks, and no impurity peaks appear, indicating that pure phase ZSM-48 and ZSM-23 molecular sieves are still obtained after repair, and the introduction of P species does not change the structure of the molecular sieve. Table 1 is the crystallinity data calculated and sorted out from the XRD spectra of the molecular sieves prepared in each embodiment and comparative example. It can be seen from Table 1 that the crystallinity of the molecular sieves in each embodiment repaired by the repair method of the present invention is significantly higher than that of the unrepaired ZSM-48 molecular sieve original powder and ZSM-23 original powder, indicating that the molecular sieve treated by the method of the present invention has a more complete physical phase structure. (Note: The crystallinity of the unrepaired ZSM-48 and unrepaired ZSM-23 molecular sieve original powders is set to 1.00).

[0106] Figure 2 is the solid NMR spectrum of L3 in Example 3 and Comparative Example 1. Figure 2 It can be seen that -105 to -110 ppm corresponds to the chemical shift of uncoordinated saturated silicon species (Si-OH), and the silicon spectrum of Example 3 repaired by the method of the present invention shows a gentle trend at the chemical shift of -105 to -110 ppm, and the peak of the uncoordinated silicon species almost completely disappears, indicating that the Si-OH in the repaired silicon-aluminum molecular sieve is transformed into a Si-O-Si structure, and the latter exhibits better hydrophobicity.

[0107] Infrared spectroscopy is one of the important methods for qualitative analysis of substances. The position of infrared absorption peaks can reflect the characteristics of molecular structures and can be used to identify the structural composition and chemical groups of substances. Figure 3is the infrared spectra of the different samples prepared above. Figure 3 It can be seen that in the FTIR images of different samples, the wave number is 475 cm -1 、550 cm -1 、793 cm -1 、1112cm -1 Corresponding to the characteristic peak of the framework structure of ZSM-48 molecular sieve, compared with the unrepaired ZSM-48 molecular sieve, the ZSM-48 molecular sieve sample in the embodiment after repair has a peak at 720 cm in the infrared spectrum. -1 Symmetrical stretching vibration peaks of PO bonds appear at all locations, indicating that after the repair treatment, the phosphorus species successfully entered the molecular sieve framework, and the introduction of phosphorus did not affect the integrity of the molecular sieve structure.

[0108] Figure 4 Together with Table 2, it is shown that, using the model compound palmitic acid as the raw material, the repaired molecular sieve catalysts in each embodiment are compared with the untreated one-dimensional ten-membered ring silica-alumina molecular sieve catalyst. Due to the reduction of the uncoordinated saturated skeleton structure of the repaired molecular sieve catalyst and the introduction of P species, the adsorption of water molecules formed in the hydrogenation reaction of palmitic acid on the molecular sieve skeleton is further inhibited, thereby significantly improving the activity of the catalyst and the yield of aviation kerosene components (C9~C16 alkanes), and the average yield of C9~C16 alkanes is above 75%.

[0109] Table 3 shows the catalytic reaction performance results of various embodiments and comparative examples using cottonseed oil and waste grease as raw materials.

[0110] Table 3 Catalytic reaction performance results of various examples and comparative examples using cottonseed oil and waste grease as raw materials

[0111]

[0112] As shown in Table 3, compared with the untreated one-dimensional ten-membered ring silicon aluminum molecular sieve catalyst, the molecular sieve catalyst in each embodiment repaired by the repair method of the present invention exhibits tolerance to high concentration oxygen-containing compounds and excellent hydrothermal stability, and the yield of the product (aviation kerosene component) in the distillation range of 150 ℃ to 300 ℃ is above 72%. This shows that the one-step hydrogenation catalyst prepared by the method of the present invention can directly use vegetable oil or waste oil in real life as a reactant for the hydrogenation reaction catalyst performance test, and has high catalytic stability and catalytic activity.

[0113] Figure 5 , Figure 6The results show that when cottonseed oil and waste grease are used as raw materials for evaluating the stability performance of the catalyst, since the catalyst repaired by the method of the present invention has higher stability and catalytic activity, in the stability performance test lasting up to 1000 h, the various performance indicators of the catalyst remain basically unchanged, and no obvious deactivation phenomenon is observed, which lays a solid foundation for its future industrial application.

Claims

1. A molecular sieve catalyst for preparing green aviation kerosene by one-step hydrogenation of biomass oil, characterized in that: A 10-membered ring silica-alumina molecular sieve comprising a noble metal, a non-noble metal additive and an organophosphorus repaired 10-membered ring silica-alumina molecular sieve; the noble metal and the non-noble metal additive are loaded on the organophosphorus repaired 10-membered ring silica-alumina molecular sieve; the noble metal in the catalyst accounts for 0.2% to 3% by weight as an element, and the non-noble metal additive accounts for 10% to 30% by weight as an element; the 10-membered ring silica-alumina molecular sieve comprises at least one of ZSM-23, ZSM-48, ZSM-22, ZSM-35 and EU-1; The method for preparing the organophosphorus repaired ten-membered ring silica-alumina molecular sieve comprises the following steps: (S1) preparing a mixed solution of small molecule organic phosphorus, fluoride and deionized water in a mass ratio of 1: (0.6-2.5): (2-45); (S2) under stirring, adding the decacyclic silica-alumina molecular sieve powder to the mixed solution prepared in step (S1) in a mass ratio of 1:(5-90) and the total mass of the decacyclic silica-alumina molecular sieve, stirring for 1-10 hours at a temperature of 30-95° C., and transferring to a reactor for hydrothermal treatment after being fully mixed; (S3) collecting the solid product obtained in the step (S2), drying it at 80-130° C. for 6-48 h, transferring it to a muffle furnace, and calcining it at a high temperature of 400-700° C. for 3-8 h to obtain an organophosphorus repaired ten-membered ring silicon aluminum molecular sieve; The small molecule organic phosphorus includes at least one of tetramethyl phosphorus bromide, tetraethyl phosphorus bromide, tetrabutyl phosphorus bromide, tetrabutyl phosphorus hydroxide, tri-n-butylphosphine oxide, and tetraphenyl phosphorus bromide; the fluoride is selected from at least one of tetrapropylammonium fluoride, calcium fluoride, sodium fluoride, tetramethylammonium fluoride, hydrogen fluoride, tetrabutylammonium fluoride, and tetraethylammonium fluoride.

2. According to claim 1, the biomass oil one-step hydrogenation to green aviation kerosene molecular sieve catalyst is characterized in that: The noble metal is one of Pt, Pd, and Ru, and the non-noble metal is one of Ni, Co, Ce, La, and Fe.

3. The method for preparing a molecular sieve catalyst for preparing green aviation kerosene by one-step hydrogenation of biomass oil according to claim 1, characterized in that: The following steps are involved: (1) uniformly mixing an extrusion aid, a binder and an organophosphorus-repaired ten-membered ring silicon-aluminum molecular sieve; (2) Add the peptizing agent and mix into a paste, stir for 0.5-2 h, and then place in a mold for extrusion molding; (3) Then, the sample obtained in step (2) is placed in an oven at 80-180°C and dried for 10-24 hours; (4) calcining at 300-600°C for 3-60 h; (5) dripping a solution containing a noble metal salt into the calcined product obtained in step (4), drying at room temperature for 1-3 h, then drying at a drying temperature of 110 °C for 12 h, and then calcining at a temperature of 550 °C for 6 h to obtain a single metal supported catalyst; (6) Then, the non-precious metal salt solution is dripped into the monometallic supported catalyst obtained in step (5), and the catalyst is dried at room temperature for 1-3 h, and then dried at 110 °C for 12 h, and then calcined at 550 °C for 6 h, thereby obtaining a biomass oil one-step hydrogenation to green aviation kerosene molecular sieve catalyst.

4. The preparation method according to claim 3, characterized in that: The mass ratio of the organic phosphorus repaired ten-membered ring silicon aluminum molecular sieve, extrusion aid, peptizing agent and binder added is 1: 0.1~5: 0.1~1.5: 0.3~2.

5. The use of the molecular sieve catalyst for preparing green aviation kerosene by one-step hydrogenation of biomass oil according to claim 1, characterized in that: Used for one-step hydrogenation of biomass oil.

6. A method for using the molecular sieve catalyst for preparing green aviation kerosene by one-step hydrogenation of biomass oil according to claim 1 for one-step hydrogenation of biomass oil, characterized in that: The method comprises using biomass oil as raw material, at a reaction temperature of 260-340°C, a hydrogen-to-oil ratio of 50-4000:1, and a liquid hourly space velocity of 0.15-6 h -1 Under the condition of a pressure of 3.5-9 Mpa, the biomass oil one-step hydrogenation to produce green aviation kerosene molecular sieve catalyst is placed in a fixed bed reactor to carry out a one-step hydrogenation reaction of the biomass oil.

Citation Information

Patent Citations

  • Catalyst for hydrogenated production of diesel oil with high cetane number by plant oil and preparation and usage methods of catalyst

    CN104998668A

  • Catalytic cracking aid including Beta molecular sieve containing phosphorus and loading metal, and preparation method thereof

    CN107971003A

  • High-stability molecular sieve and n-alkane hydroisomerization catalyst prepared from high-stability molecular sieve

    CN116835606A

  • Manufacturing method of AEI type zeolite

    JP2017039638A