Preparation method of modified high-strength aluminum-based powder based on selective laser melting nano ceramic

The composite powder of nano-TiB2 ceramic powder and Al-20Si alloy powder is prepared through selective laser melting technology and high-energy ball milling process, which solves the problems of organizational continuity and stress concentration during the forming process of high-strength aluminum alloy materials, and achieves a significant improvement in the mechanical properties of the material. and improvements in production efficiency.

CN118699401APending Publication Date: 2024-09-27NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411036246.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-09-27

AI Technical Summary

Technical Problem

Traditional high-strength aluminum alloy materials have problems such as fragmentation of organizational continuity, stress concentration and crack initiation during the forming process, resulting in a decrease in material strength and elongation. The rapid solidification method is complex and expensive, making it difficult to form complex parts using powder metallurgy processes.

Method used

Selective laser melting technology is combined with high-energy ball milling technology to prepare composite powder of nano-TiB2 ceramic powder and Al-20Si alloy powder. The morphology and distribution of the silicon phase are adjusted through selective laser melting forming technology to improve the mechanical properties of the material.

Benefits of technology

It significantly improves the mechanical properties of high-strength aluminum alloys, shortens the production cycle, reduces costs, and can form parts with complex geometric shapes. There is almost no need for subsequent machining. The material structure is dense, and cracks and pore defects are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118699401A
    Figure CN118699401A
Patent Text Reader

Abstract

The invention discloses a preparation method of modified high-strength aluminum-based powder based on selective laser melting nano ceramics. According to the method, nanoscale titanium diboride (TiB2) ceramic powder is meticulously prepared by adopting a high-energy ball milling process. And high-purity high-strength aluminum alloy powder and the prepared nano titanium diboride powder are mixed to be completely uniform through a ball mill under the protection of inert gas, and the novel nano ceramic modified high-strength aluminum alloy powder is formed. Advanced selective laser melting forming equipment is utilized, the powder is accurately melted and solidified layer by layer, and a needed target part is constructed. In the process, the nanometer titanium diboride powder serves as an effective heterogeneous nucleation point, and precipitation and growth of a silicon phase in the solidification process are remarkably hindered. The mechanical property of the high-strength aluminum alloy can be remarkably improved. The innovation not only enhances the strength and toughness of the material, but also provides new possibility for the use of the high-strength aluminum alloy in the high-performance application field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of high-strength aluminum alloy materials, and in particular, relates to a method for preparing high-strength aluminum-based powder modified by nano-ceramics based on selective laser melting. Background Art

[0002] High-strength aluminum alloys have the advantages of low density, high strength, good corrosion resistance, and low thermal expansion coefficient. They have great development potential and extremely broad application prospects in the fields of automobiles, aerospace, and electronic packaging. Unlike hypoeutectic and eutectic aluminum-silicon alloys, the silicon phase in the hypereutectic high-strength aluminum alloy structure exists in two forms: primary silicon phase and eutectic silicon phase. With the increase of silicon content, the wear resistance and heat resistance of aluminum alloys are improved, but the size, morphology and distribution of primary silicon and eutectic silicon phases in the microstructure of the formed parts also have a significant impact on their mechanical properties, especially the coarse lamellar primary silicon phase in the traditional casting structure seriously breaks the continuity of the organization, and stress concentration is easily generated at the edges and sharp parts of the silicon phase, which increases the crack initiation points, and finally reduces the strength and elongation of the material. Based on this, nano-ceramic phases are added to the aluminum matrix for structural modification, increasing the heterogeneous nucleation points during the solidification of aluminum melt, effectively adjusting the morphology, size and distribution of primary silicon phase and eutectic silicon phase, and finally achieving the purpose of improving the mechanical properties of the material. Among the common ceramic phases used to modify aluminum alloys, titanium diboride has higher elastic modulus (560GPa) and hardness (35GPa), excellent heat resistance and wear resistance, and good wettability with the aluminum matrix, which makes titanium diboride an ideal structural modification material in high-strength aluminum alloys.

[0003] From the perspective of processing technology, in order to achieve the purpose of grain refinement, uniform structure and improved mechanical properties of materials, rapid solidification methods such as spray deposition and powder metallurgy are usually used to prepare hypereutectic high-strength aluminum alloys. However, the equipment and process of spray deposition are relatively complex, and the production cost is relatively high. The parts made by powder metallurgy have a high internal porosity and it is difficult to form parts with more complex structures. Summary of the invention

[0004] In view of the problems existing in the current high-strength aluminum alloy material preparation technology and to meet the improvement needs proposed above, the present invention provides a preparation method of high-strength aluminum-based powder modified by selective laser melting of nano-ceramics, so as to significantly improve the mechanical properties of high-strength aluminum alloy.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] The preparation method of nano-ceramic modified high-strength aluminum-based powder based on selective laser melting includes the following steps:

[0007] (1) Nano-TiB2 ceramic powder was prepared by Pulverisette 6 single-tank planetary high-energy ball milling process;

[0008] (2) mixing the Al-20Si alloy powder and the nano-TiB2 ceramic powder prepared in step (1) uniformly by using a QM series planetary ball mill under the protection of an inert gas to obtain a nano-TiB2 / Al-20Si composite powder;

[0009] (3) Use Soildworks software to build a 3D solid geometric model of the target part in a computer, then use Magics software to slice the model and plan the laser scanning path, discretize the 3D solid into a series of 2D data, save the file and import it into the selective laser melting forming equipment;

[0010] (4) The selective laser melting forming equipment melts the nano-TiB2 / Al-20Si composite powder in step (2) layer by layer according to the file saved in step (3) to form the target part to be built.

[0011] Preferably, in step (1), the raw material used is polygonal micron TiB2 powder with a particle size distribution range of 1 to 5 μm and a purity greater than 99.9%.

[0012] Preferably, in step (1), the high-energy ball milling speed is 250 to 300 rpm and the ball milling time is 20 to 25 hours.

[0013] Preferably, in step (1), the particle size of the nano-TiB2 ceramic powder prepared by high-energy ball milling is 40 to 200 nm.

[0014] Preferably, in step (2), the Al-20Si alloy powder has a particle size distribution range of 12 to 31 μm, wherein the silicon content is 19.2 to 20 wt.%, the iron content is 0.05 to 0.15%, and the balance is aluminum.

[0015] Preferably, in step (2), the content of nano-TiB2 particles in the TiB2 / Al-20Si composite powder is 1 to 10 wt.%, most preferably 2 wt.%. If the content of nano-TiB2 particles is too low, the modification effect is poor; if the content of nano-TiB2 particles is too high, the laser forming quality is reduced, affecting the performance of the composite material.

[0016] Specifically, in step (2), the ball mill adopts a QM series planetary ball mill for ball milling and powder mixing operation. The process adopts a ceramic jar, and the ball milling medium is a ceramic grinding ball with a diameter of 6 mm and 8 mm. The ball milling process parameters are set as follows: the ball-to-material ratio is 2:1; at the same time, in order to prevent the temperature in the ball mill from being too high, the equipment operation mode during ball milling is selected as an interval type, that is, the equipment is suspended for air cooling for 5 minutes after every 15 minutes of operation. The ball milling process is required to be carried out under the protection of inert gas to prevent the aluminum alloy powder from being oxidized or contaminated.

[0017] Preferably, in step (2), the ball milling speed is 150-250 rpm and the ball milling time is 3-5 h.

[0018] Specifically, step (4) uses an SLM-150 selective laser melting device, which mainly includes a YLR-500 fiber laser, a laser forming chamber, an automatic powder spreading system, a protective atmosphere device, a computer control circuit system, and a cooling circulation system. Before forming, the sandblasted aluminum substrate is fixed on the workbench of the selective laser melting forming device and leveled, and then the forming chamber is sealed, evacuated, and an inert gas protective atmosphere is introduced through a sealing device. The typical selective laser melting forming process is as follows: (a) The powder spreading device evenly spreads the powder to be processed on the forming substrate, and the laser beam scans the slicing area line by line according to a pre-designed scanning path, so that the powder layer undergoes rapid melting-solidification, thereby obtaining the first two-dimensional plane of the part; (b) The computer control system causes the forming substrate to drop a powder layer thickness, and conversely, causes the powder supply cylinder piston to rise a powder layer thickness, and the powder spreading device re-lays a layer of powder to be processed, and the laser beam completes the second powder layer scanning according to the slicing information to obtain the second two-dimensional plane of the part; (c) Repeat the above steps, and the powder to be processed is formed layer by layer until the part is processed.

[0019] Preferably, the laser scanning speed of the selected area laser melting forming in step (4) is 1800-2200 mm / s, the laser power is 450 W, the scanning interval is 50 μm, the powder thickness is 50 μm, and a partitioned island scanning strategy is adopted. The above laser parameters are determined after process optimization.

[0020] According to the microstructure and performance characteristics of high-strength aluminum alloy materials, high-strength aluminum alloy structural modifiers can be reasonably selected and appropriately added, and a preparation method combined with cutting-edge laser additive manufacturing technology can be adopted to effectively adjust the morphology, size and distribution state of the silicon phase, and successfully prepare high-strength aluminum alloy materials with excellent comprehensive performance.

[0021] Compared with the prior art, the present invention adopts the above technical solution and has the following beneficial effects:

[0022] (1) In the present invention, micron-sized titanium diboride powder is used as raw material, and nano-TiB2 powder is prepared by high-energy ball milling process. The prepared nano-TiB2 is mixed with Al-20Si powder and then placed in a QM series planetary ball mill for ball milling. By optimizing the ball milling process, a TiB2 / Al-20Si composite powder with uniform nano-TiB2 distribution and good flowability suitable for selective laser melting is finally obtained. The process is simple to operate and saves costs.

[0023] (2) Compared with Al-20Si alloy powder, the laser absorption rate of nano-TiB2 / Al-20Si powder is significantly increased. During the selective laser melting process, the laser energy input to the powder bed increases, so that the powder layer can be fully melted, thereby improving the forming quality of the parts.

[0024] (3) The present invention uses selective laser melting technology to prepare high-strength aluminum alloy materials, which not only shortens the production cycle and improves product production efficiency, but also can form parts with complex geometric shapes with almost no subsequent machining. The cooling rate of the molten pool during selective laser melting is extremely high, reaching 103-108K / s, which increases the supercooling of the high-strength aluminum alloy melt, avoids the formation of coarse dendrites in traditional processing technology, and improves the mechanical properties of the parts.

[0025] (4) During the solidification process of TiB2 / Al-20Si melt, nano-TiB2 increases the heterogeneous nucleation points of silicon phase precipitation, hinders the growth of silicon phase precipitated at the front of the solidifying liquid phase, significantly reduces the star-shaped primary silicon phase, blunts the edges of the polygonal primary silicon phase, smoothes the edges, and significantly refines the fibrous eutectic silicon structure. The present invention can effectively adjust the morphology and distribution state of the primary silicon phase and the eutectic silicon phase in the high-strength aluminum alloy structure through the refinement and modification of nano-TiB2 on the primary silicon phase and the eutectic silicon phase, and significantly improves the mechanical properties of Al-20Si.

[0026] (5) The optimal laser power for selective laser melting of high-strength aluminum alloys was obtained through preliminary process optimization, and the laser energy density was adjusted by changing the laser scanning speed. As the laser energy input of the powder bed changes, the thermodynamic and kinetic characteristics of the molten pool formed by the interaction between the laser and the powder bed also change. By reasonably selecting laser process parameters and adjusting the laser energy input, the generation of metallurgical defects such as spheroidization effect, pores, and cracks is reduced, and a TiB2 / Al-20Si composite material with dense organization and good comprehensive performance is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 TEM image of nano-TiB2 prepared by high-energy ball milling process in Example 1;

[0028] Figure 2 This is a SEM image of the TiB2 / Al-20Si composite powder obtained in Example 3;

[0029] Figure 3 This is a physical photo of the sample of the selective laser melted nano-TiB2 / Al-20Si composite material obtained in Example 3;

[0030] Figure 4 This is a SEM image of the nano-TiB2 / Al-20Si composite material sample formed by selective laser melting in Example 3;

[0031] Figure 5 This is the SEM image of the Al-20Si alloy sample formed by selective laser melting in Comparative Example 1;

[0032] Figure 6 This is the SEM image of the micron TiB2 / AlSi10Mg composite material sample formed by selective laser melting in Comparative Example 3. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] In the following examples, the TiB2 powder raw material used is polygonal micron TiB2 powder with a particle size distribution range of 1 to 5 μm and a purity greater than 99.9%. The Al-20Si alloy powder has a particle size of 12 to 31 μm, wherein the silicon content is 19.2 to 20 wt.%, the iron content is 0.11%, and the balance is aluminum.

[0035] Example 1

[0036] (1) Nano-TiB2 ceramic powder was prepared by high-energy ball milling process. The high-energy ball milling equipment was a Pulverisette 6 single-tank planetary high-energy ball mill. The ball milling media in the stainless steel ball mill were stainless steel grinding balls with diameters of 6 mm and 20 mm, and the ball-to-material ratio was 10:1. When the equipment was working, the stainless steel ball mill rotated around its own axis at a fixed speed, and at the same time revolved around a fixed axis parallel to its own axis. The ball milling speed was set to 250 rpm, and the ball milling time was 25 hours. During the high-energy ball milling process, the grinding balls and ceramic powder collided and impacted each other, causing the ceramic phase particles to break, thereby obtaining nano-TiB2 ceramic powder. The TEM image of the nano-TiB2 powder prepared by this high-energy ball milling process is shown in the following figure. Figure 1 shown.

[0037] (2) The nano-TiB2 ceramic powder prepared in step (1) is added to the Al-20Si alloy powder at a ratio of 1wt%, and the powder is mixed by ball milling to prepare TiB2 / Al-20Si composite powder. The ball milling and mixing operation is carried out in a QM series planetary ball mill. The process uses a ceramic jar and the ball milling medium is ceramic grinding balls with diameters of 6mm and 8mm. The ball milling process parameters are set as follows: ball-to-material ratio is 2:1, ball milling speed is 150rpm, and ball milling time is 5h. At the same time, in order to prevent the temperature in the ball mill jar from being too high, the equipment operation mode during ball milling is selected as interval type, that is, the equipment is suspended for air cooling for 5min after every 15min of operation. The ball milling process is required to be carried out under argon protection to prevent the aluminum alloy powder from being oxidized or contaminated.

[0038] (3) Target part modeling and slicing

[0039] The 3D solid geometric model of the target part was established using Soildworks software in the computer, and then the 3D solid model was sliced ​​and scanned using Magics software, and the 3D solid was discretized into a series of 2D data. The file was saved and imported into the selective laser melting forming equipment. The laser process parameters were set as follows: laser power of 450W, laser scanning speed of 1800mm / s, scanning spacing of 50μm, powder thickness of 50μm, partitioned island scanning strategy, and the rotation angle of the laser scanning direction of adjacent layers was 37°.

[0040] (4) Selective laser melting process

[0041] The nano-ceramic modified high-strength aluminum alloy powder prepared in step (2) is used for selective laser melting. The SLM-150 selective laser melting equipment is used, and the system mainly includes a YLR-500 fiber laser, a laser forming chamber, an automatic powder spreading system, a protective atmosphere device, a computer control circuit system and a cooling circulation system. Before forming, the sandblasted aluminum substrate is fixed on the workbench of the selective laser melting forming equipment and leveled, and then the forming cavity is sealed, evacuated and introduced into an argon protective atmosphere (argon purity is 99.999%, outlet pressure is 30mbar) through a sealing device to ensure that the O2 content in the forming chamber is less than 10ppm. The typical selective laser melting forming process is as follows: (a) The powder spreading device evenly spreads the powder to be processed on the forming substrate, and the laser beam scans the slicing area line by line according to the pre-designed scanning path, so that the powder layer is quickly melted and solidified, thereby obtaining the first two-dimensional plane of the part; (b) The computer control system causes the forming substrate to drop by one powder layer thickness, and conversely, causes the piston of the powder supply cylinder to rise by one powder layer thickness. The powder spreading device re-spreads a layer of powder to be processed, and the laser beam completes the second powder layer scan according to the slicing information to obtain the second two-dimensional plane of the part; (c) Repeat the above steps, and the powder to be processed is formed layer by layer until the part is processed.

[0042] After cooling, the formed substrate is taken out of the equipment, and the parts are separated from the substrate by wire cutting process to obtain the nano-titanium diboride modified high-strength aluminum alloy sample. The nano-titanium diboride modified high-strength aluminum alloy block sample is ground, polished and corroded according to the standard metallographic sample preparation method.

[0043] The obtained TiB2 / Al-20 Si standard tensile specimen was subjected to room temperature tensile test, and its tensile strength could reach 409MPa.

[0044] Example 2

[0045] (1) Nano-TiB2 ceramic powder was prepared by high-energy ball milling process. The high-energy ball milling equipment was a Pulverisette 6 single-tank planetary high-energy ball mill. The ball milling medium in the stainless steel ball mill was stainless steel grinding balls with diameters of 6 mm and 20 mm, and the ball-to-material ratio was 10:1. When the equipment was working, the stainless steel ball mill rotated around its own axis at a fixed speed, and at the same time, it revolved around a fixed axis parallel to its own axis. The ball milling speed was set to 280 rpm, and the ball milling time was 23 h. During the high-energy ball milling process, the grinding balls and ceramic powder collided and impacted each other to break the ceramic phase particles, thereby obtaining nano-TiB2 ceramic powder.

[0046] (2) The nano-TiB2 ceramic powder prepared in step (1) is added to the Al-20Si alloy powder at a ratio of 10wt.%, and the powder is mixed by ball milling to prepare TiB2 / Al-20Si composite powder. The ball milling and mixing operation is carried out in a QM series planetary ball mill. The process uses a ceramic jar and the ball milling medium is a ceramic grinding ball with a diameter of 6mm and 8mm. The ball milling process parameters are set as follows: the ball-to-material ratio is 2:1, the ball milling speed is 200rpm, and the ball milling time is 4h. At the same time, in order to prevent the temperature in the ball mill jar from being too high, the equipment operation mode during ball milling is selected as the interval type, that is, the equipment is suspended for air cooling for 5min after every 15min of operation. The ball milling process is required to be carried out under argon protection to prevent the aluminum alloy powder from being oxidized or contaminated.

[0047] (3) Target part modeling and slicing

[0048] The 3D solid geometric model of the target part was established using Soildworks software in the computer, and then Magics software was used to perform layered slicing and scanning path planning on the 3D solid model, discretizing the 3D solid into a series of 2D data, saving this file and importing it into the selective laser melting forming equipment. The laser process parameters were set as follows: laser power of 450W, laser scanning speed of 2000mm / s, scanning spacing of 50μm, powder thickness of 50μm, partitioned island scanning strategy, and the rotation angle of the laser scanning direction of adjacent layers was 37°.

[0049] (4) Selective laser melting process

[0050] The nano-ceramic modified high-strength aluminum alloy powder prepared in step (2) is used for selective laser melting. The SLM-150 selective laser melting equipment is used, and the system mainly includes a YLR-500 fiber laser, a laser forming chamber, an automatic powder spreading system, a protective atmosphere device, a computer control circuit system and a cooling circulation system. Before forming, the sandblasted aluminum substrate is fixed on the workbench of the selective laser melting forming equipment and leveled, and then the forming cavity is sealed, evacuated and introduced into an argon protective atmosphere (argon purity is 99.999%, outlet pressure is 30mbar) through a sealing device to ensure that the O2 content in the forming chamber is less than 10ppm. The typical selective laser melting forming process is as follows: (a) The powder spreading device evenly spreads the powder to be processed on the forming substrate, and the laser beam scans the slicing area line by line according to the pre-designed scanning path, so that the powder layer is quickly melted and solidified, thereby obtaining the first two-dimensional plane of the part; (b) The computer control system causes the forming substrate to drop by one powder layer thickness, and conversely, causes the piston of the powder supply cylinder to rise by one powder layer thickness. The powder spreading device re-spreads a layer of powder to be processed, and the laser beam completes the second powder layer scan according to the slicing information to obtain the second two-dimensional plane of the part; (c) Repeat the above steps, and the powder to be processed is formed layer by layer until the part is processed.

[0051] After cooling, the formed substrate is taken out of the equipment, and the parts are separated from the substrate by wire cutting process to obtain the nano-titanium diboride modified high-strength aluminum alloy sample. The nano-titanium diboride modified high-strength aluminum alloy block sample is ground, polished and corroded according to the standard metallographic sample preparation method.

[0052] The obtained TiB2 / Al-20Si standard tensile specimen was subjected to room temperature tensile test, and its tensile strength could reach 472MPa.

[0053] Example 3

[0054] (1) Nano-TiB2 ceramic powder was prepared by high-energy ball milling process. The high-energy ball milling equipment was a Pulverisette 6 single-tank planetary high-energy ball mill. The ball milling medium in the stainless steel ball mill was stainless steel grinding balls with diameters of 6 mm and 20 mm, and the ball-to-material ratio was 10:1. When the equipment was working, the stainless steel ball mill rotated around its own axis at a fixed speed, and at the same time, it revolved around a fixed axis parallel to its own axis. The ball milling speed was set to 300 rpm, and the ball milling time was 20 hours. During the high-energy ball milling process, the grinding balls and ceramic powder collided and impacted each other to break the ceramic phase particles, thereby obtaining nano-TiB2 ceramic powder.

[0055] (2) Add the nano-TiB2 ceramic powder obtained in step (1) to the Al-20Si alloy powder at a ratio of 2wt.%, and perform ball milling to prepare TiB2 / Al-20Si composite powder. The ball milling and powder mixing operation is performed in a QM series planetary ball mill. The process uses a ceramic jar and the ball milling media are ceramic grinding balls with diameters of 6mm and 8mm. The ball milling process parameters are set as follows: ball-to-material ratio is 2:1, ball milling speed is 250rpm, and ball milling time is 3h. At the same time, in order to prevent the temperature in the ball mill jar from being too high, the equipment operation mode is selected as the interval type during ball milling, that is, the equipment is suspended for air cooling for 5 minutes after every 15 minutes of operation. The ball milling process is required to be carried out under argon protection to prevent the aluminum alloy powder from being oxidized or contaminated. The SEM image of the nano-TiB2 / Al-20Si powder prepared by the ball milling and powder mixing is shown in the figure. Figure 2 shown.

[0056] (3) Target part modeling and slicing

[0057] The 3D solid geometric model of the target part was established using Soildworks software in the computer, and then the 3D solid model was sliced ​​and scanned using Magics software, and the 3D solid was discretized into a series of 2D data. The file was saved and imported into the selective laser melting forming equipment. The laser process parameters were set as follows: laser power of 450W, laser scanning speed of 2200mm / s, scanning spacing of 50μm, powder thickness of 50μm, partitioned island scanning strategy, and the rotation angle of the laser scanning direction of adjacent layers was 37°.

[0058] (4) Selective laser melting process

[0059] The nano-ceramic modified high-strength aluminum alloy powder prepared in step (2) is used for selective laser melting. The SLM-150 selective laser melting equipment is used, and the system mainly includes a YLR-500 fiber laser, a laser forming chamber, an automatic powder spreading system, a protective atmosphere device, a computer control circuit system and a cooling circulation system. Before forming, the sandblasted aluminum substrate is fixed on the workbench of the selective laser melting forming equipment and leveled, and then the forming cavity is sealed, evacuated and introduced into an argon protective atmosphere (argon purity is 99.999%, outlet pressure is 30mbar) through a sealing device to ensure that the O2 content in the forming chamber is less than 10ppm. The typical selective laser melting forming process is as follows: (a) The powder spreading device evenly spreads the powder to be processed on the forming substrate, and the laser beam scans the slicing area line by line according to the pre-designed scanning path, so that the powder layer is quickly melted and solidified, thereby obtaining the first two-dimensional plane of the part; (b) The computer control system causes the forming substrate to drop by one powder layer thickness, and conversely, the piston of the powder supply cylinder rises by one powder layer thickness. The powder spreading device re-lays a layer of powder to be processed, and the laser beam completes the second powder layer scan according to the slicing information to obtain the second two-dimensional plane of the part; (c) Repeat the above steps, and the powder to be processed is formed layer by layer until the part is processed. Figure 3 The microstructure of the nano-TiB2 / Al-20Si composite material sample prepared by the selective laser melting process is shown in Figure 2. Figure 4 shown.

[0060] After cooling, the formed substrate is taken out of the equipment, and the parts are separated from the substrate by wire cutting process to obtain the nano-titanium diboride modified high-strength aluminum alloy sample. The nano-titanium diboride modified high-strength aluminum alloy block sample is ground, polished and corroded according to the standard metallographic sample preparation method. The microstructure morphology of the nano-TiB2 / Al-20Si composite material sample in this example is as follows: Figure 4 shown.

[0061] The obtained TiB2 / Al-20Si standard tensile specimen was subjected to room temperature tensile test, and its tensile strength can reach 494MPa

[0062] Comparative Example 1

[0063] This comparative example relates to a method for preparing a high-strength aluminum-based powder modified by nano-ceramic by selective laser melting. The specific steps are basically the same as those of Example 3, except that: in steps (1) and (2) of this comparative example, nano-TiB2 raw material is not used to prepare nano-TiB2 / Al-20Si composite powder by ball milling process, but nearly spherical Al-20Si alloy powder prepared by gas atomization is used as raw material for selective laser melting forming. Its microstructure is as follows: Figure 5 As shown. Figure 4 and Figure 5It can be found that compared with the nano-TiB2 / Al-20Si composite material, the number of star-shaped and polygonal primary silicon phases in the Al-20Si alloy structure is significantly increased and the dispersion is uneven, showing an aggregated state, while the size of the fibrous eutectic silicon is significantly increased. Stress concentration is prone to occur in the brittle silicon phase aggregation area or the polygonal edges of the larger primary silicon phase, resulting in premature crack generation and expansion, thereby reducing the mechanical properties of the material.

[0064] The Al-20Si alloy standard tensile specimen prepared in step (3) is subjected to a room temperature tensile test, and its tensile strength can reach 357 MPa.

[0065] Comparative Example 2

[0066] This comparative example relates to a preparation method of a high-strength aluminum-based powder modified by selective laser melting of nano-ceramic. The specific steps are basically the same as those of Example 3, except that in step (2) of this comparative example, the content of TiB2 nanoparticles in the nano-TiB2 / Al-20Si composite powder is 25wt.%. In this comparative example, due to the excessive addition of nano-TiB2 ceramics, the nanoparticles agglomerate and significantly increase the viscosity of the aluminum melt. In the subsequent solidification process, the gaps between the powder particles lack sufficient melt filling to form pore defects, thereby causing the forming quality and performance of the sample to be seriously reduced.

[0067] Comparative Example 3

[0068] This comparative example relates to a method for preparing a high-strength aluminum-based powder modified by selective laser melting of nano-ceramic. The specific steps are basically the same as those of Example 3, except that: in steps (1) and (2) of this comparative example, micron TiB2 and AlSi10Mg alloy powders are used as raw materials, a ball milling process is used to prepare a 2wt.% TiB2 / AlSi10Mg composite powder, and selective laser melting is performed to form the composite powder. The microstructure thereof is as follows: Figure 6 As shown. Figure 4 and Figure 6 It can be found that the eutectic silicon structure in the micron TiB2 / AlSi10Mg composite material is significantly coarsened compared with the nano-TiB2 / Al-20Si composite material. This is mainly because the micron ceramic phase has a weaker degree of refinement of the aluminum-based composite material structure than the nano-ceramic phase; at the same time, the larger ceramic phase increases the tendency of internal stress concentration and fracture of the material. The aluminum alloy used in this example has a low silicon content (lower than the eutectic point of aluminum-silicon alloy 12.6wt.%), and no uniformly distributed small block primary silicon phase is precipitated during the solidification of the aluminum alloy melt, thereby reducing the strength of the composite material.

[0069] The tensile strength of the TiB2 / AlSi10Mg composite material measured by room temperature tensile test is 444MPa. It can be seen from Examples 1 to 3 and Comparative Examples 1 to 3 that the tensile strength of the nano-TiB2 / Al-20Si composite material sample formed by selective laser melting is significantly increased, and the mechanical properties are significantly improved, which is mainly attributed to the refinement and modification of the primary silicon phase and eutectic silicon phase in the high-strength aluminum alloy structure by nano-TiB2. Compared with the Al-20Si alloy, the star-shaped primary silicon phase in the nano-TiB2 / Al-20Si composite material is significantly reduced, the edges of the polygonal primary silicon phase are blunted, the edges are smooth, and the fibrous eutectic silicon structure is significantly refined. Nano-TiB2 is evenly distributed on the aluminum matrix, which plays a dispersion strengthening role on the high-strength aluminum alloy matrix, and the wettability of TiB2 ceramics and aluminum alloys is good, so that the interface between the nano-TiB2 ceramic phase and the aluminum matrix is ​​tightly bonded, further improving the mechanical properties of the material.

[0070] The present invention provides a method for preparing a high-strength aluminum-based powder modified by selective laser melting of nano-ceramic. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.

Claims

1. A method for preparing high-strength aluminum-based powder modified by nano-ceramic by selective laser melting, characterized in that: Prepared by the following steps: (1) Nano-TiB2 ceramic powder was prepared using a Pulverisette 6 single-tank planetary high-energy ball mill; (2) mixing the Al-20Si alloy powder and the nano-TiB2 ceramic powder prepared in step (1) uniformly by using a QM series planetary ball mill under the protection of an inert gas to obtain a nano-TiB2 and Al-20Si composite powder; (3) Use Soildworks software to build a 3D solid geometric model of the target part in a computer, then use Magics software to slice the model and plan the laser scanning path, discretize the 3D solid into a series of 2D data, save the file and import it into the selective laser melting forming equipment; (4) The selective laser melting forming equipment melts the nano-TiB2 and Al-20Si composite powders in step (2) layer by layer according to the file saved in step (3), and finally forms the target part to be built.

2. The method for preparing high-strength aluminum-based powder modified by selective laser melting of nano-ceramics according to claim 1 is characterized in that: In the step (1), the raw material used is polygonal micron TiB2 powder with a particle size distribution range of 1 to 5 μm and a purity greater than 99.9%.

3. The method for preparing high-strength aluminum-based powder modified by selective laser melting of nano-ceramics according to claim 1, characterized in that: In the step (1), the high-energy ball milling speed is 250-300 rpm, and the ball milling time is 20-25 hours.

4. The method for preparing high-strength aluminum-based powder modified by selective laser melting of nano-ceramics according to claim 3 is characterized in that: In the step (1), the particle size of the nano-TiB2 ceramic powder prepared by high-energy ball milling is 40 to 200 nm.

5. The method for preparing high-strength aluminum-based powder modified by selective laser melting of nano-ceramics according to claim 1, characterized in that: In step (2), the Al-20Si alloy powder has a particle size distribution range of 12 to 31 μm, wherein the silicon content is 19.2 to 20 wt.%, the iron content is 0.05 to 0.15%, and the balance is aluminum.

6. The method for preparing high-strength aluminum-based powder modified by selective laser melting of nano-ceramics according to claim 1, characterized in that: In step (2), the content of TiB2 nanoparticles in the nano-TiB2 and Al-20Si composite powder is 1 to 10 wt.%.

7. The method for preparing high-strength aluminum-based powder modified by selective laser melting of nano-ceramics according to claim 1, characterized in that: In the step (2), the ball milling speed is 150-250 rpm, and the ball milling time is 3-5 h.

8. The method for preparing high-strength aluminum-based powder modified by selective laser melting of nano-ceramics according to claim 1, characterized in that: In the step (4), the laser scanning speed used in the selective laser melting is 1800 to 2200 mm / s.

Citation Information

Cited By

  • Porous high-compactness aluminum-based composite material and preparation method thereof

    CN121467696A