Coating material and preparation method thereof, positive electrode material and preparation method thereof, sodium ion battery

The wet coating process forms a cage-like structured cladding material, which solves the stability and cycle times of the positive electrode material of sodium ion battery, improves the cycle life and energy density of the battery, and is suitable for industrial production.

CN118702138BActive Publication Date: 2024-12-03GANZHOU NOVA TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411170056.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing sodium ion battery positive electrode materials are prone to moisture, have poor air stability, and have poor phase change properties, which limits the structural stability and number of cycles of the material.

Method used

Using the wet coating process, a cage-like coating material is formed by the reaction of hydrated zeolite and metal salt solution, and combined with sodium sulfide solution to form a sulfide coating layer such as ZnS or CuS, which enhances the structural stability of the positive electrode material. and sodium ion storage capacity.

Benefits of technology

It improves the cycle life and energy density of sodium ion batteries, enhances the structural stability and conductivity of the positive electrode material, reduces interface side reactions, broadens research ideas and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118702138B_ABST
    Figure CN118702138B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of sodium ion battery materials, and discloses a method for preparing a coating material for a positive electrode material of a sodium ion battery, including hydrating zeolite; adding a metal salt solution to the hydrated zeolite, heating, stirring, and obtaining slurry I; the activity of the metal in the metal salt is weaker than that of sodium; separating the slurry I from the solid and liquid, washing and drying the obtained solid phase to obtain a powder; hydrating the powder; adding a sodium sulfide solution to the hydrated powder, heating, stirring, and obtaining slurry II; separating the slurry II from the solid and liquid, washing and drying the obtained solid phase, and obtaining a coating material. In addition, the present invention claims protection for the coating material prepared by the above-mentioned preparation method, as well as the sodium ion battery positive electrode material coated and modified by the coating material, and claims protection for a battery comprising the sodium ion battery positive electrode material coated and modified by the coating material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion battery materials, and in particular relates to the coating modification of positive electrode materials of sodium ion batteries. Background Art

[0002] Sodium-ion batteries are secondary batteries that rely on the movement of sodium ions between the positive and negative electrodes to work, similar to the working principle of lithium-ion batteries. Compared with lithium-ion batteries, sodium-ion batteries have cost advantages and have received much attention and favor from researchers.

[0003] In terms of key performance of sodium-ion batteries such as energy density and number of cycles, positive electrode materials play a very critical role. Generally, positive electrode materials need to have the characteristics of high specific capacity (affecting energy density), abundant resources (affecting cost), stable structure (the structure does not undergo phase change or the phase change is highly reversible during the sodium ion insertion and extraction process) and high operating voltage (affecting energy density). At present, ordinary positive electrode materials are easily affected by moisture, have poor air stability, and are prone to adverse effects. At present, the key points of research on positive electrode materials for sodium-ion batteries are mainly focused on how to improve air stability, reduce interfacial side reactions, inhibit phase changes to achieve high structural reversibility, etc. The commonly used research strategy is coating. At present, the commonly used coating method mostly uses solid-phase coating of coating materials. Due to the characteristics of the coating materials and the uneven coating, the improvement of the material structure stability is greatly limited. Summary of the invention

[0004] In view of the problems existing in the prior art, the first object of the present invention is to provide a coating material for a sodium ion battery positive electrode material and a preparation method thereof; the second object of the present invention is to provide a sodium ion battery positive electrode material and a preparation method thereof; the third object of the present invention is to provide a sodium ion battery.

[0005] First, the present invention provides a method for preparing a coating material for a sodium ion battery positive electrode material, comprising the following steps:

[0006] Step S1, hydrating zeolite;

[0007] Step S2, adding a metal salt solution to the hydrated zeolite, heating, and stirring to obtain slurry I; the metal in the metal salt is less active than sodium;

[0008] Step S3, separating the slurry I from the solid and liquid, and washing and drying the obtained solid phase to obtain a powder;

[0009] Step S4, hydrating the powder;

[0010] Step S5, adding sodium sulfide solution to the hydrated powder, heating, stirring, and obtaining slurry II;

[0011] Step S6, separating the slurry II from the solid and liquid, and washing and drying the obtained solid phase to obtain the coating material.

[0012] The hydration described in the present invention refers to keeping in deionized water for a period of time.

[0013] In a further preferred embodiment, in step S1, 5-15 g of zeolite is added to every 50 mL of water.

[0014] It is further preferred that the time for hydrating the zeolite is 9-15 hours.

[0015] In a further preferred embodiment, the metal salt is one or both of zinc sulfate and copper sulfate.

[0016] It is further preferred that the concentration of the metal salt solution is 0.05-0.3 mol / L.

[0017] In a further preferred embodiment, the solid-liquid ratio of the hydrated zeolite to the metal salt solution is 5-15 g:150 mL.

[0018] In a further preferred embodiment, in step S4, when the powder is hydrated, the solid-liquid ratio is 1-10 g:50 ml; and the time for hydrating the powder is 8-16 h.

[0019] In a further preferred embodiment, the concentration of the sodium sulfide solution is 0.05-0.3 mol / L.

[0020] In a further preferred embodiment, the solid-liquid ratio of the hydrated powder to the sodium sulfide solution is 1-10 g:150 mL.

[0021] In a further preferred embodiment, the heating temperature in step S2 and step S5 is 30-70°C.

[0022] In a further preferred embodiment, the drying temperature in step S3 and step S6 is 30-40°C.

[0023] In a further preferred embodiment, the stirring time in step S2 is 30-80 min; the stirring time in step S5 is 30-80 min.

[0024] Based on the same inventive concept, the present invention further provides a coating material prepared by the above preparation method.

[0025] Secondly, the present invention provides a sodium ion battery positive electrode material, including a positive electrode material matrix and the above-mentioned coating material located on the surface of a portion of the positive electrode material matrix.

[0026] In a further preferred embodiment, the cathode material matrix is ​​NaNi x Fe yMn 1-x-y O2, where 0.2≤x≤0.5, 0.1≤y≤0.4.

[0027] In a further preferred embodiment, the mass ratio of the coating material to the positive electrode material matrix is ​​1-5:100.

[0028] In addition, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising the following steps:

[0029] Dispersing the cathode material matrix and the coating material in ethanol, stirring, heating, and then drying the materials;

[0030] The sodium ion battery positive electrode material is obtained by calcining and drying the material.

[0031] In a further preferred embodiment, the heating temperature is 50-120°C.

[0032] In a further preferred embodiment, the drying temperature is 100-130°C.

[0033] In a further preferred embodiment, the calcination temperature is 300-450° C. and the calcination time is 2-4 hours.

[0034] Based on the same inventive concept, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode material.

[0035] Compared with the prior art, the above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects:

[0036] The present invention provides a more novel coating material for lithium ion battery positive electrode materials, broadening the research ideas.

[0037] The process for preparing the coating material of the present invention is simple, the raw materials are easily available, and the coating material is very suitable for industrial production.

[0038] The sodium ion battery provided by the invention has a relatively good cycle life and a relatively high capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The schematic diagram of the preparation of the coating material of the present invention is shown in FIG.

[0040] Figure 2 These are SEM images of the positive electrode materials before and after coating of Example 1 of the present invention, wherein Figure (a) is the SEM image of the positive electrode material before coating, and Figure (b) is the SEM image of the positive electrode material after coating.

[0041] Figure 3 The positive electrode materials and NaNi prepared in each embodiment 1 / 3 Fe 1 / 3 Mn1 / 3 O2、NaNi 0.4 Fe 0.4 Mn 0.2 Cycling performance diagram of batteries with O2 as the positive electrode material. DETAILED DESCRIPTION

[0042] At present, the modification of positive electrode materials of sodium ion batteries is restricted by coating materials and solid-phase coating processes. The present invention provides a more novel coating material and can adopt a wet coating process when modifying and coating the positive electrode material.

[0043] First, the present invention provides a method for preparing a coating material, comprising the following steps:

[0044] Step S1, hydrating zeolite;

[0045] Step S2, adding a metal salt solution to the hydrated zeolite, heating, and stirring to obtain slurry I; the metal in the metal salt is less active than sodium;

[0046] Step S3, separating the slurry I from the solid and liquid, and washing and drying the obtained solid phase to obtain a powder;

[0047] Step S4, hydrating the powder;

[0048] Step S5, adding sodium sulfide solution to the hydrated powder, heating, stirring, and obtaining slurry II;

[0049] Step S6, separating the slurry II from the solid and liquid, and washing and drying the obtained solid phase to obtain the coating material.

[0050] The schematic diagram of the process of preparing the coating material is as follows Figure 1 shown.

[0051] The microstructure of zeolite is cage-like with a hole in the center of the unit cell. When zinc sulfate solution is added to the cage-like zeolite, the surface of the cage-like zeolite will adsorb Zn ions (or other metal ions with weaker metal activity than sodium). Then Na2S solution is further added. 2- It passes through the zeolite cage to the center and reacts with Zn ions (or other metal ions with weaker metal activity than sodium) to form ZnS nanoparticles (or corresponding sulfide particles of other metals), while Na + The ions return to their original positions in the zeolite cage. The final structure of the material is a zeolite cage with ZnS (or the corresponding sulfide of other metals) in the center, and the outer cage is composed of the sodium, aluminum, silicon, oxygen and other elements of the zeolite itself.

[0052] In the present invention, the hydration refers to keeping in deionized water for a period of time.

[0053] In some specific embodiments of the present invention, in step S1, 5-15 g of zeolite is added to every 50 mL of water; and the time for hydrating the zeolite is 9-15 h.

[0054] In some specific embodiments of the present invention, the metal salt is preferably one or both of zinc sulfate and copper sulfate.

[0055] In some specific embodiments of the present invention, the concentration of the metal salt solution is 0.05-0.3 mol / L, such as 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L.

[0056] In some specific embodiments of the present invention, the solid-to-liquid ratio of the hydrated zeolite to the metal salt solution is 5-15 g:150 mL.

[0057] In some specific embodiments of the present invention, in step S4, when the powder is hydrated, the solid-liquid ratio is 1-10 g:150 mL and the time is 8-16 h.

[0058] In some specific embodiments of the present invention, the concentration of the sodium sulfide solution is 0.05-0.3 mol / L, such as 0.05 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L.

[0059] In some specific embodiments of the present invention, the solid-to-liquid ratio of the hydrated powder to the sodium sulfide solution is 5 g:150 mL.

[0060] In some specific embodiments of the present invention, the heating temperature in step S2 and step S5 is 30-70°C, such as 30°C, 40°C, 50°C, 60°C, 70°C, etc.

[0061] In some specific embodiments of the present invention, the drying temperature in step S3 and step S6 is 30-40° C. Low-temperature drying is beneficial to maintaining the structural stability of the product.

[0062] In some specific embodiments of the present invention, the stirring time in step S2 is 30-80 min; the stirring time in step S5 is 30-80 min.

[0063] The present invention further provides a coating material prepared by the above preparation method.

[0064] Secondly, the present invention provides a sodium ion battery positive electrode material, including a positive electrode material matrix and the above-mentioned coating material located on the surface of a portion of the positive electrode material matrix.

[0065] In some specific embodiments of the present invention, the cathode material matrix is ​​NaNi x Fey Mn 1-x-y O2, where 0.2≤x≤0.5, 0.1≤y≤0.4.

[0066] In some specific embodiments of the present invention, the mass ratio of the coating material to the positive electrode material matrix is ​​1-5:100.

[0067] In addition, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising the following steps:

[0068] Dispersing the cathode material matrix and the coating material in ethanol, stirring, heating, and then drying the materials;

[0069] The sodium ion battery positive electrode material is obtained by calcining and drying the material.

[0070] The coating material is first coated on the surface of the positive electrode material through a wet process, and the coating layer is more uniform and closely fits the positive electrode material. At the same time, from a theoretical analysis: because the coating material has a cage-like structure, it can increase the sodium ion storage capacity of the positive electrode material, and the cage-like structure is also conducive to the structural stability of the positive electrode material. The ZnS (including other metal sulfides such as CuS) in the core position can also play a certain catalytic role, catalyzing the conversion of sodium ions, enhancing conductivity, and thus increasing the cycle life and capacity of the battery.

[0071] In some specific embodiments of the present invention, the heating temperature is 50-120°C.

[0072] In some specific embodiments of the present invention, the drying temperature is 100-130°C.

[0073] In some specific embodiments of the present invention, the calcination temperature is 300-450°C and the calcination time is 2-4 hours. By calcining, the coating material is attached to the surface of the core material, which can make its distribution more uniform on the one hand and make the structure after coating more stable and not easy to fall off during the circulation process on the other hand.

[0074] Some embodiments of the present invention also provide a sodium ion battery comprising the above-mentioned positive electrode material.

[0075] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0076] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0077] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0078] Embodiment 1:

[0079] Step (1): First, 10 g of zeolite was placed in 50 mL of deionized water for 12 h to hydrate it and obtain hydrated zeolite. At the same time, 150 mL of 0.1 mol / L ZnSO4 solution was prepared.

[0080] Step (2): 150 mL of a 0.1 mol / L ZnSO4 solution was mixed with the above hydrated zeolite, heated to 50°C, and magnetically stirred for 50 min to mix evenly to obtain a slurry.

[0081] Step (3): Filter the slurry, wash the filtered solid phase three times with deionized water, and dry it at room temperature (35°C in summer) to obtain powder I.

[0082] Step (4): The obtained powder I is placed in 50 ml of deionized water for 16 h to hydrate it and obtain hydrated powder I.

[0083] Step (5): Mix 150 mL of 0.1 mol / L Na2S solution with the above hydrated powder I, heat to 50°C, and stir magnetically for 50 min to mix evenly to obtain a slurry. Filter the slurry, wash the filtered solid phase three times with deionized water, and then dry at room temperature (35°C in summer) to obtain powder II.

[0084] Step (6): 10g of positive electrode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is dispersed in 100 mL of anhydrous ethanol, and then 0.5 g of powder II is added, stirred, placed in an oil bath to evaporate the ethanol, and then thoroughly dried in an oven at 120°C, where the oil bath temperature can be 50-120°C.

[0085] Step (7): The material obtained in step (6) is calcined in a muffle furnace at 400° C. for 3 h to obtain a coated modified sodium ion battery positive electrode material.

[0086] Figure 2 For uncoated NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 From the SEM images of the coated and modified positive electrode materials obtained in Example 1, it can be found that the layered structure of the layered oxide surface before coating is more obvious, with more obvious edges and corners, while the surface of the positive electrode material after coating is slightly passivated and small particles appear, indicating that it has been successfully coated.

[0087] Embodiment 2:

[0088] Step (1): First, 10 g of zeolite was placed in 100 mL of deionized water for 9 h to hydrate it and obtain hydrated zeolite.

[0089] Step (2): 150 mL of a 0.2 mol / L ZnSO4 solution was mixed with the above hydrated zeolite, heated to 60°C, and magnetically stirred for 30 min to mix evenly to obtain a slurry.

[0090] Step (3): Filter the slurry, wash the filtered solid phase three times with deionized water, and dry it at room temperature (35°C in summer) to obtain powder I.

[0091] Step (4): The obtained powder I is placed in 50 ml of deionized water for 8 h to hydrate it and obtain hydrated powder I.

[0092] Step (5): Mix 150 mL of 0.2 mol / L Na2S solution with the above hydrated powder I, heat to 70°C, and stir magnetically for 50 min to obtain a slurry. Filter the slurry, wash the filtered solid phase three times with deionized water, and then dry at room temperature (35°C in summer) to obtain powder II.

[0093] Step (6): 10g of positive electrode material NaNi 0.4 Fe 0.4 Mn 0.2 O2 is dispersed in 100 mL of anhydrous ethanol, and then 0.3 g of powder II is added, stirred, placed in an oil bath to evaporate the ethanol, and then thoroughly dried in an oven at 120°C, where the oil bath temperature can be 50-120°C.

[0094] Step (7): The material obtained in step (6) is calcined in a muffle furnace at 450° C. for 2 h to obtain a coated modified sodium ion battery positive electrode material.

[0095] Embodiment 3:

[0096] Step (1): First, 15 g of zeolite was dissolved in 50 mL of deionized water for 12 h to hydrate the zeolite and simultaneously 150 mL of 0.3 mol / L ZnSO4 solution was prepared.

[0097] Step (2): 150 mL of a 0.3 mol / L ZnSO4 solution was mixed with the above hydrated zeolite, heated to 70°C, and magnetically stirred for 50 min to mix evenly to obtain a slurry.

[0098] Step (3): Filter the slurry, wash the filtered solid phase three times with deionized water, and dry it at room temperature (35°C in summer) to obtain powder I.

[0099] Step (4): The obtained powder I is placed in 150 ml of deionized water for 12 h to hydrate it and obtain hydrated powder I.

[0100] Step (5): Mix 150 mL of 0.3 mol / L Na2S solution with the above hydrated powder I, heat to 70°C, and stir magnetically for 50 min to obtain a slurry. Filter the slurry, wash the filtered solid phase three times with deionized water, and then dry at room temperature (35°C in summer) to obtain powder II.

[0101] Step (6): 10g of positive electrode material NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2 is dispersed in 100 mL of anhydrous ethanol, and then 0.1 g of powder II is added, stirred, placed in an oil bath to evaporate the ethanol, and then thoroughly dried in an oven at 120°C, where the oil bath temperature can be 50-120°C.

[0102] Step (7): The material obtained in step (6) is calcined in a muffle furnace at 300° C. for 3 h to obtain a coated modified sodium ion battery positive electrode material.

[0103] Example 4

[0104] Step (1): First, 10 g of zeolite was dissolved in 50 mL of deionized water for 15 h to hydrate it and obtain hydrated zeolite.

[0105] Step (2): 150 mL of a 0.1 mol / L CuSO4 solution was mixed with the above hydrated zeolite, heated to 50° C., and magnetically stirred for 50 min to mix evenly to obtain a slurry.

[0106] Step (3): Filter the slurry, wash the filtered solid phase three times with deionized water, and dry it at room temperature (35°C in summer) to obtain powder I.

[0107] Step (4): The obtained powder I is placed in 50 ml of deionized water for 15 h to hydrate it and obtain hydrated powder I.

[0108] Step (5): Mix 150 mL of 0.1 mol / L Na2S solution with the above hydrated powder I, heat to 50°C, and stir magnetically for 50 min to obtain a slurry. Filter the slurry, wash the filtered solid phase three times with deionized water, and then dry at room temperature (35°C in summer) to obtain powder II.

[0109] Step (6): 10g of positive electrode material NaNi 0.4 Fe 0.4 Mn 0.2 O2 is dispersed in 100 mL of anhydrous ethanol, and then 0.5 g of powder II is added, stirred, placed in an oil bath to evaporate the ethanol, and then thoroughly dried in a 120 ℃ oven, where the oil bath temperature can be 50-120 ℃.

[0110] Step (7): The material obtained in step (6) is calcined in a muffle furnace at 400° C. for 3 h to obtain a coated modified sodium ion battery positive electrode material.

[0111] The positive electrode materials obtained in Examples 1-4 and the uncoated NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2、NaNi 0.4 Fe 0.4 Mn 0.2 O2 was weighed and ground according to the ratio of positive electrode material: conductive graphite: PVDF of 8:1:1, dissolved in an appropriate amount of N-methylpyrrolidone (NMP) and stirred evenly to form a slurry, and then the slurry was coated on the current collector aluminum foil, dried at 90°C for 12 h in a blast dryer, and punched into a disc electrode with a diameter of 12 mm. The disc electrode was used as the positive electrode, the metal sodium sheet was used as the negative electrode, 1 mol / L NaPF6 / EC+DEC+DMC (EC:DEC:DMC=1:1:1 volume ratio) was used as the electrolyte, and GF / D sodium electrolyte was used as the separator. The button cell was assembled in the glove box according to the assembly order of the button cell.

[0112] The electrical performance of the battery was tested in the following manner: operating voltage range 2.0-4.0 V, current density 1C, and 50 cycles.

[0113] The battery cycle performance data are shown in Table 1 and Figure 3 As shown, it can be seen that the coated and modified positive electrode material can make the battery have a slightly higher capacity retention rate and cycle stability than the uncoated and modified positive electrode material.

[0114] Table 1

[0115]

[0116] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A sodium ion battery cathode material, It is characterized in that It comprises a positive electrode material substrate and a coating layer located on at least a portion of the surface of the positive electrode material substrate, wherein the material of the coating layer is prepared according to the following preparation method: Step S1, hydrating zeolite; Step S2, adding a metal salt solution to the hydrated zeolite, heating, and stirring to obtain slurry I; the metal in the metal salt is less active than sodium; Step S3, separating the slurry I from the solid and liquid, and washing and drying the obtained solid phase to obtain a powder; Step S4, hydrating the powder; Step S5, adding sodium sulfide solution to the hydrated powder, heating, stirring, and obtaining slurry II; Step S6, separating the slurry II into solid and liquid, washing and drying the obtained solid phase, and obtaining the coating layer material.

2. The sodium ion battery positive electrode material according to claim 1, It is characterized in that In step S1: 5-15 g of zeolite is added to every 50 mL of water; the hydration time of the zeolite is 9-15 hours; In step S2: the concentration of the metal salt solution is 0.05-0.3 mol / L; the metal salt is one or both of zinc sulfate and copper sulfate; the solid-liquid ratio of the hydrated zeolite to the metal salt solution is 5-15 g:150 mL.

3. The sodium ion battery positive electrode material according to claim 1, It is characterized in that In step S4: when the powder is hydrated, the solid-liquid ratio is 1-10 g:50 ml; the time for hydrating the powder is 8-16 hours; In step S5: the concentration of the sodium sulfide solution is 0.05-0.3 mol / L; the solid-liquid ratio of the hydrated powder to the sodium sulfide solution is 5-15 g:150 mL.

4. The sodium ion battery positive electrode material according to any one of claims 1 to 3, It is characterized in that The heating temperature in step S2 and step S5 is 30-70°C; the drying temperature in step S3 and step S6 is 30-40°C; the stirring time in step S2 is 30-80min; and the stirring time in step S5 is 30-80min.

5. The sodium ion battery positive electrode material according to claim 1, It is characterized in that The positive electrode material matrix is ​​NaNi x Fe y Mn 1-x-y O 2 , wherein 0.2≤x≤0.5, 0.1≤y≤0.4; the mass ratio of the material of the coating layer to the positive electrode material matrix is ​​1-5:

100.

6. The method for preparing the positive electrode material for a sodium ion battery according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Dispersing the positive electrode material matrix and the coating layer material in ethanol, stirring, heating, and then drying the materials; The sodium ion battery positive electrode material is obtained by calcining and drying the material.

7. The preparation method according to claim 6, It is characterized in that The heating temperature is 50-120° C.; the drying temperature is 100-130° C.; the calcining temperature is 300-450° C.; and the calcining time is 2-4 hours.

8. A sodium ion battery, It is characterized in that The invention comprises the sodium ion battery positive electrode material according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Modified sodium ion battery positive electrode material, preparation method thereof and sodium ion battery

    CN117117158A