Zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass, preparation method and equipment

The zirconia catalyst was prepared by using UiO-66(Zr) template agent and high-temperature calcination stepwise method, which solved the problems of low yield and strong corrosiveness of existing catalysts in pyrolysis biomass, and realized efficient and environmentally friendly 5-hydroxyl Catalytic effect of methylfurfural.

CN118702144AInactive Publication Date: 2024-09-27ANHUI UNIVERSITY OF ARCHITECTURE

Patent Information

Application Number
CN202410514959.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-09-27
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing catalysts have low yields for releasing 5-hydroxymethylfurfural in pyrolysis biomass, and have problems such as high toxicity, strong corrosion to equipment, and unfavorable recovery.

Method used

UiO-66(Zr) is used as a metal template, and the zirconia catalyst is prepared in stages through high-temperature carbonization and high-temperature calcination. Its specific surface area and structure are controlled to form a loose and porous nano-needle structure to improve catalytic activity.

Benefits of technology

The content of 5-hydroxymethylfurfural in pyrolyzed biomass is significantly increased. The catalyst is easy to recycle, has good environmental performance and low cost, and is suitable for increasing the yield of 5-HMF in biomass derivatives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118702144A
    Figure CN118702144A
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of zirconium oxide catalytic materials, in particular to a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural through biomass pyrolysis and a preparation method and device.UiO-66 (Zr) is adopted as a metal template agent, an inorganic zirconium source and organic ligand powder are selected to be dissolved in an acid mixed solution of N, N-dimethylformamide (DMF), and the zirconium oxide catalytic material is prepared; the preparation method comprises the following steps: adding an acid mixed solution and a dissolved and dispersed mixed solution into a polytetrafluoroethylene reaction kettle, carrying out stirring and ultrasonic treatment on the acid mixed solution, adding the dissolved and dispersed mixed solution into the polytetrafluoroethylene reaction kettle, carrying out centrifugation or suction filtration treatment on a reaction product after the reaction is finished, washing, drying and activating a precipitate obtained by treatment to finally obtain UiO-66 (Zr) powder, putting the UiO-66 (Zr) powder into a tubular furnace, and carrying out ultrasonic treatment on the UiO-66 (Zr) powder to obtain the UiO-66 (Zr) powder. The zirconium oxide solid acid catalyst obtained by sectional high-temperature carbonization-high-temperature calcination can obviously improve the content of 5-hydroxymethylfurfural released by biomass pyrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of zirconium oxide catalytic material preparation, and in particular to a zirconium oxide catalytic material for pyrolyzing biomass to release 5-hydroxymethylfurfural, a preparation method and equipment. Background Art

[0002] Catalytic pyrolysis is becoming one of the important technologies for processing and utilizing biomass energy due to its low operating cost. Catalytic pyrolysis of biomass is a very complex process that produces a series of derivatives, such as biochar, bio-oil, oxygen heterocyclic compounds, etc. As an important type of oxygen heterocyclic compound, 5-hydroxymethylfurfural (5-HMF) is an aromatic and environmentally friendly organic compound that can be derived into a series of high value-added compounds through hydrogenation, oxidation, condensation and other reactions, playing an important role in the synthesis of biofuels, chemical raw materials and fine chemicals.

[0003] At present, catalysts play a key role in improving the yield of biomass derivative 5-HMF by pyrolysis catalysis. Acidic catalysts can selectively catalyze esterification reactions, thereby having good directional catalytic effects on the preparation of oxygen heterocyclic compounds by pyrolysis of biomass, including inorganic acids and organic acids, such as H2SO4 and HCl inorganic acid catalysts, but they have problems such as high toxicity, strong corrosion to equipment, inconvenience in recovery, complex product composition and low yield. Therefore, it is particularly important to develop environmentally friendly and efficient solid acid catalysts, which have the advantages of good catalytic activity, easy recovery and low corrosion, such as zeolite molecular sieves, ion exchange resins, metal oxides, etc. Among them, metal oxide catalysts have attracted widespread attention due to their important influence on catalytic activity due to their specific surface area, stability and particle size. The preparation of common metal oxide catalysts is mainly prepared by simple modification or direct calcination of metal salts, which has problems such as difficult to control the size of the specific surface area and easy agglomeration of the catalyst, resulting in low catalytic efficiency. Therefore, the controllable preparation method and equipment optimization of catalysts with high specific surface area and high active sites are still a technical problem. Summary of the invention

[0004] In view of this, the purpose of the present invention is to propose a zirconium oxide catalytic material, preparation method and equipment for pyrolyzing biomass to release 5-hydroxymethylfurfural, so as to solve the problem that the content of 5-hydroxymethylfurfural released by pyrolyzing biomass with existing catalytic materials needs to be further improved.

[0005] Based on the above purpose, the present invention provides a method for preparing a zirconium oxide catalytic material for pyrolyzing biomass to release 5-hydroxymethylfurfural, comprising the following steps:

[0006] S1: preparing UiO-66 (Zr) sacrificial template agent, dissolving inorganic zirconium source and organic ligand powder in an acid mixture of N, N-dimethylformamide (DMF), stirring and ultrasonically treating the acid mixture until the inorganic zirconium source and organic ligand powder are completely dissolved and dispersed, adding the dissolved and dispersed mixed solution into a polytetrafluoroethylene reactor, reacting at 110°C to 150°C for 20 to 28 hours, and after the reaction, centrifuging or filtering the reaction product, washing the obtained precipitate with DMF and anhydrous ethanol for 3 times, respectively, drying and activating the washed precipitate, and finally obtaining UiO-66 (Zr) powder;

[0007] S2 calcination is used to prepare zirconium oxide catalytic material. The selected UiO-66 (Zr) powder is placed in a tubular furnace and calcined in stages under nitrogen and air atmospheres, respectively. The calcination temperature is 500-800°C and the temperature is kept for 3-5 hours to obtain a porous zirconium oxide catalytic material ZrO2.

[0008] Preferably, the selected inorganic zirconium source and organic ligand powder are ZrCl4 and terephthalic acid, the mass ratio of ZrCl4 and terephthalic acid is 1.2:1 to 1.5:1, the acid mixture includes N, N-dimethylformamide (DMF) and glacial acetic acid, the volume ratio of N, N-dimethylformamide and glacial acetic acid is 5:1 to 9:1, and the dissolved and dispersed mixed solution is added to a polytetrafluoroethylene reactor for reaction.

[0009] Preferably, the washed precipitate is dried at 100° C. for 12 h, and then vacuum dried at 150° C. for activation for 3 h, to finally obtain UiO-66(Zr) white powder.

[0010] Preferably, the selected UiO-66 (Zr) powder is placed in a tubular furnace, heated to 500-800°C at a heating rate of 5°C / min in a nitrogen atmosphere, and kept warm for 2 hours, and then calcined in an air atmosphere and kept warm for 2 hours to obtain zirconium oxide catalytic material ZrO2.

[0011] The present invention also provides a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass, which is prepared by the above method for preparing the zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass.

[0012] Preferably, the zirconium oxide catalytic material has a loose porous structure formed by a combination of nano needles, wherein the thickness of the nano needle structure is 30-50nm, the length is 200nm-800nm, and the specific surface area is 35-70m 2 / g.

[0013] The present invention also provides a preparation device for a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass, comprising a filtering centrifuge main body, the filtering centrifuge main body comprising an upper cover assembly, a body assembly, and a drum assembly, the body assembly comprising a base, a casing fixed on the base, a drum driving device at the bottom of the casing, and a liquid outlet at the bottom of the casing, the drum assembly comprising a drum arranged in the casing, and the upper cover assembly comprising an upper cover hinged to the top of the casing, an observation mirror at the top of the upper cover, and a feed pipe at the top of the upper cover:

[0014] A movable ring net is arranged around the inner side of the drum, and a ring top plate is arranged around the top of the movable ring net. A movable lifting inner material pipe is inserted into the feed pipe, and a horizontal stirring blade is arranged on the lower side wall of the inner material pipe, and a horizontal limiting blade is arranged on the upper side wall of the inner material pipe. The inner material pipe moves upward until the top of the horizontal stirring blade abuts against the ring top plate, driving the ring top plate to move up, and the movable ring net moves up against the inner side of the drum, so that the mesh of the movable ring net is opposite to the mesh of the drum, and the drum rotates rapidly in a centrifugal mode;

[0015] It moves downward through the inner material pipe until the horizontal stirring blade extends into the bottom of the drum, and the bottom end of the horizontal limiting blade abuts against the annular top plate, driving the annular top plate to move downward, and the movable ring net moves downward close to the inner side of the drum, so that the mesh of the movable ring net is misaligned with the mesh of the drum, and the drum rotates slowly in washing mode.

[0016] Preferably, a through hole is opened on one end of the annular top plate near the movable ring network, and a movable block is slidably connected in the annular top plate, and an elastic member is connected between the movable block and the movable block, and the movable block is pushed outward by the elastic member to close the through hole of one end of the movable block, and an upper limit block, a middle limit block and a lower limit block are fixed on the inner side wall of the rotating drum from top to bottom in sequence, and the middle limit block is designed in a rectangular shape at one end near the rotating drum, and the upper and lower end surfaces of the middle limit block away from the rotating drum are designed with inclined end surfaces, and the upper and lower ends of the annular top plate are elastically connected with movable rings at the upper and lower ends of the annular top plate, respectively. When the horizontal stirring blade abuts against the annular top plate, the movable ring at the lower end is pushed to drive the movable block to slide inward and compress the elastic member until the movable block moves to the inclined end surface of the upper end of the middle limit block, and the horizontal stirring blade stops moving up, and the movable block is pushed by the elastic member to make the movable block slide along the inclined end surface of the upper end, driving the annular top plate to move between the upper limit block and the middle limit block, and the rotating drum rotates rapidly in a centrifugal mode;

[0017] When the transverse limiting leaf abuts against the annular top plate, it pushes the movable ring at the upper end, drives the movable block to slide inward, and compresses the elastic member until the movable block moves to the inclined end surface of the lower end of the middle limiting block. The transverse limiting leaf stops moving downward, and pushes the movable block through the elastic member, so that the movable block slides along the inclined end surface of the lower end, drives the annular top plate to move between the lower limiting block and the middle limiting block, and the drum rotates slowly to enter the washing mode;

[0018] The movable ring net is provided with avoidance holes at positions below the perforations, which are used for avoiding the upper limit block, the middle limit block and the lower limit block.

[0019] Preferably, a connecting rope is connected between the movable block and the movable ring, and when the movable ring is pressed inward, the movable block is driven to move inward laterally through the connecting rope.

[0020] Preferably, an air inlet pipe is connected to the bottom end of the upper cover for spraying heated gas toward the inside of the drum, and the drum rotates rapidly in a drying mode.

[0021] The beneficial effects of the present invention are as follows: by using UiO-66 (Zr) as a metal template and utilizing a high-temperature carbonization-high-temperature calcination staged method to obtain a zirconium oxide solid acid catalyst, compared to a direct calcination method, the high-temperature carbonization-high-temperature calcination staged method can make full use of the skeleton structure of UiO-66 (Zr) and thus regulate the specific surface area of ​​the catalyst. The obtained catalyst has a looser structure, is not easy to agglomerate, has a good catalytic effect, and can significantly increase the content of 5-hydroxymethylfurfural in pyrolysis biomass derivatives. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 This is the XRD pattern of UiO-66(Zr) obtained in Example 1 of the present invention;

[0024] Figure 2 This is a SEM image of UiO-66(Zr) obtained in Example 1 of the present invention;

[0025] Figure 3 The results obtained in Example 1 and Comparative Example 1 of the present invention are a ZrO2 and b XRD pattern of ZrO2;

[0026] Figure 4 The results obtained in Example 1 and Comparative Example 1 of the present invention are a ZrO2 and b SEM image of ZrO2;

[0027] Figure 5 The results obtained in Example 1 and Comparative Example 1 of the present invention are a ZrO2 and b Nitrogen adsorption and desorption data of ZrO2;

[0028] Figure 6The results obtained in Example 1 and Comparative Example 1 of the present invention are a ZrO2 and b Pore ​​size distribution diagram of ZrO2;

[0029] Figure 7 The results obtained in Example 1 and Comparative Example 1 of the present invention are a ZrO2 and b Catalytic performance diagram of ZrO2;

[0030] Figure 8 It is a schematic diagram of the overall structure of the present invention;

[0031] Fig. 9 It is a schematic structural diagram of the rotary drum of the present invention in a washing mode;

[0032] Fig.10 It is a structural schematic diagram of the rotary drum of the present invention in a centrifugal mode;

[0033] Fig.11 It is a schematic diagram of the top view of the annular top plate of the present invention;

[0034] Fig.12 For the present invention Fig.11 The enlarged schematic diagram of point A in the middle;

[0035] Fig.13 It is a schematic diagram of the structure when the transverse limiting blade of the present invention moves downward and approaches the annular top plate;

[0036] Fig.14 It is a structural schematic diagram of the present invention when the transverse limiting leaf moves downward to press the movable ring;

[0037] Fig.15 It is a structural schematic diagram when the end of the movable block of the present invention moves to the inclined end surface of the lower end of the middle limit block;

[0038] Fig.16 It is a schematic structural diagram of the annular top plate of the present invention when it moves between the lower limit block and the middle limit block.

[0039] The markings in the figure are:

[0040] 1. Centrifuge body; 2. Base; 3. Casing; 4. Drum drive device; 5. Liquid outlet; 6. Drum; 7. Upper cover; 8. Observation mirror; 9. Feed pipe; 10. Movable ring net; 11. Annular top plate; 12. Inner material pipe; 13. Horizontal stirring blade; 14. Horizontal limit blade; 15. Perforation; 16. Movable block; 17. Elastic part; 18. Upper limit block; 19. Middle limit block; 20. Lower limit block; 21. Movable ring; 22. Connecting rope; 23. Inlet pipe. DETAILED DESCRIPTION

[0041] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0042] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0043] A method for preparing a zirconium oxide catalytic material for pyrolyzing biomass to release 5-hydroxymethylfurfural comprises the following steps:

[0044] S1: preparing UiO-66 (Zr) sacrificial template agent, dissolving inorganic zirconium source and organic ligand powder in an acid mixture of N, N-dimethylformamide (DMF), stirring and ultrasonically treating the acid mixture until the inorganic zirconium source and organic ligand powder are completely dissolved and dispersed, adding the dissolved and dispersed mixed solution into a polytetrafluoroethylene reactor, reacting at 110°C to 150°C for 20 to 28 hours, and after the reaction, centrifuging or filtering the reaction product, washing the obtained precipitate with DMF and anhydrous ethanol for 3 times, respectively, drying and activating the washed precipitate, and finally obtaining UiO-66 (Zr) powder;

[0045] S2 calcination is used to prepare zirconium oxide catalytic material. The selected UiO-66 (Zr) powder is placed in a tubular furnace and calcined in stages under nitrogen and air atmospheres, respectively. The calcination temperature is 500-800°C and the temperature is kept for 3-5 hours to obtain a porous zirconium oxide catalytic material ZrO2.

[0046] Among them, metal organic framework materials (MOFs) are used to catalyze the increase of 5-HMF content in biomass derivatives due to their excellent specific surface area, high porosity, and adjustable structure, such as MIL-101 (Cr), UiO-66 (Zr), etc. Studies have shown that metal oxides prepared by MOFs as sacrificial templates can maintain a certain large specific surface area, which can make the metal Lewis acid sites in the metal oxides more evenly distributed, and have been used in other catalytic reactions. Therefore, MOFs materials can be used as sacrificial templates to prepare metal oxides, and the specific surface area and active sites of the catalyst can be regulated by certain means, thereby catalyzing the pyrolysis of biomass to increase the content of 5-HMF in the derivatives.

[0047] Embodiment 1:

[0048] First, 0.0725g ZrCl4 and 0.0541g terephthalic acid were dissolved in a mixed solution of 35ml DMF and 5ml glacial acetic acid, and ultrasonic treatment was performed for 30min until ZrCl4 and terephthalic acid powders were completely dissolved and dispersed, and then the mixed solution was added to a 60ml polytetrafluoroethylene reactor and reacted at 120°C for 24h. After the reaction was completed, it was cooled to room temperature, and the obtained product was centrifuged. The white precipitate obtained after centrifugation was washed three times with DMF and anhydrous ethanol respectively, and the final precipitate was dried at 100°C for 12h, and then vacuum dried at 150°C for activation for 3h, and finally UiO-66(Zr) white powder was obtained.

[0049] A certain amount of UiO-66 (Zr) white powder was placed in a tube furnace, heated to 500 °C at a heating rate of 5 °C / min in a nitrogen atmosphere, and kept at this temperature for 2 h. Then, it was calcined in an air atmosphere and kept at this temperature for 2 h. The obtained zirconium oxide was recorded as b ZrO2.

[0050] Comparative Example 1:

[0051] First, 0.0725g ZrCl4 and 0.0541g terephthalic acid were dissolved in a mixed solution of 35ml DMF and 5ml glacial acetic acid, and ultrasonic treatment was performed for 30min until ZrCl4 and terephthalic acid powders were completely dissolved and dispersed, and then the mixed solution was added to a 60ml polytetrafluoroethylene reactor and reacted at 120°C for 24h. After the reaction was completed, it was cooled to room temperature, and the obtained product was centrifuged. The white precipitate obtained after centrifugation was washed three times with DMF and anhydrous ethanol respectively, and the final precipitate was dried at 100°C for 12h, and then vacuum dried at 150°C for activation for 3h, and finally UiO-66(Zr) white powder was obtained.

[0052] A certain amount of UiO-66 (Zr) white powder was placed in a tube furnace and heated to 500°C at a heating rate of 5°C / min in an air atmosphere for calcination. The obtained zirconium oxide was recorded as a ZrO2.

[0053] a ZrO2 and b The specific surface area, average pore diameter and total pore volume of the ZrO2 catalyst are shown in the following table:

[0054] Table 1 a ZrO2 and b Specific surface area, average pore size and total pore volume of ZrO2 catalyst

[0055]

[0056] The evaluation results of the above catalyst pyrolysis experiment are as follows:

[0057] (1) Direct pyrolysis of biomass without catalyst

[0058] 1 mg of biomass was directly filled into a pyrolysis quartz tube filled with quartz wool, and then quartz wool was laid on top of the biomass. CDS was directly pyrolyzed without catalyst at 500°C, and the content of the gas produced by pyrolysis was analyzed online by GC / MS. The chromatographic peaks were identified according to the NIST spectral library. The content of 5-hydroxymethylfurfural in the pyrolysis biomass derivative without catalyst was obtained as a blank reference.

[0059] (2) a Evaluation of the catalytic performance of ZrO2

[0060] 1mg biomass and 1mg a The ZrO2 catalyst is sequentially filled into the pyrolysis quartz tube filled with quartz wool, and then the biomass and zirconium oxide solid acid catalyst are mechanically mixed, and finally quartz wool is laid on the top of the mixture to prevent the escape of solid particles. The rapid pyrolysis temperature is raised to 500°C, and the content of the gas produced by pyrolysis is analyzed online by GC / MS, and the chromatographic peaks are identified according to the NIST spectral library.

[0061] (3) b Evaluation of the catalytic performance of ZrO2

[0062] 1mg biomass and 1mg b The ZrO2 catalyst was sequentially filled into the pyrolysis quartz tube filled with quartz wool, and then the biomass and zirconium oxide solid acid catalyst were mechanically mixed, and finally quartz wool was laid on the mixture. The rapid pyrolysis temperature was raised to 500°C, and the content of the gas produced by pyrolysis was analyzed online by GC / MS, and the chromatographic peaks were identified according to the NIST spectral library.

[0063] The experiment was performed at least three times under each reaction condition. For each pyrolysis product on the chromatogram, its peak area and peak area percentage value were recorded. In order to avoid the influence of the mass of the pyrolysis sample, the peak area was normalized by dividing it by the initial mass of the loaded biomass. The peak area percentage of each pyrolysis product was used to determine the pyrolysis change of the product, and the peak area percentage values ​​were compared to determine the concentration change between the detected pyrolysis products, and to determine the catalytic efficiency of the zirconium oxide solid acid catalyst in biomass pyrolysis.

[0064] The reaction evaluation results are as follows Figure 7 As shown. Figure 7 It can be seen from the data that the zirconia solid acid catalyst prepared by the present invention has a good catalytic effect and has a very obvious effect on the catalytic pyrolysis of biomass to increase the yield of 5-hydroxymethylfurfural in the derivatives. The catalytic effects of the two zirconia solid acid catalysts are compared with the direct pyrolysis of 1 mg of biomass, and the yield of 5-hydroxymethylfurfural is improved. However, b The catalytic effect of ZrO2 catalyst is significantly better than a ZrO2. It shows that the excellent specific surface area of ​​the zirconium oxide solid acid catalyst obtained by high-temperature carbonization-high-temperature calcination staged method using UiO-66 (Zr) as a metal template is beneficial to improving the reaction activity of the catalyst. The zirconium oxide solid acid catalyst is prepared by high-temperature carbonization-high-temperature calcination staged method. Since high-temperature carbonization can maintain the carbon skeleton structure of UiO-66 (Zr) to a certain extent, the porous skeleton structure of UiO-66 (Zr) can be fully utilized. Then the high-temperature calcination oxidation process will change the pore structure characteristics, so the pore structure and specific surface area of ​​the metal oxide can be regulated. To a certain extent, the crystal structure, morphology and size of the metal oxide can be controlled, thereby regulating the performance of the material. The results show that although the surface of the solid acid catalyst obtained by the two methods is needle-pricked flower clusters and the structure is fluffy, the one prepared by high-temperature carbonization-high-temperature calcination staged method is b ZrO2 solid acid catalyst has a large specific surface area, and the agglomeration phenomenon is not obvious. It can expose more metal Lewis acid active sites, which is more conducive to the adsorption of organic matter in biomass, improve the catalytic effect of the catalyst, and significantly increase the content of biomass derivative 5-hydroxymethylfurfural. The catalyst is not only easy to recycle, but also further broadens the application of MOFs materials in catalytic pyrolysis of biomass to increase the release of 5-HMF content. b ZrO2 catalyst is expected to show better performance in catalyzing the pyrolysis of biomass to increase the 5-hydroxymethylfurfural content in the derivatives.

[0065] In summary, the zirconium oxide solid acid catalyst provided by the present invention can be used to catalyze the pyrolysis of biomass to increase the content of released 5-hydroxymethylfurfural, and the applicable process conditions are mild, will not cause corrosion to the equipment, has high catalytic performance, and the catalyst is green and environmentally friendly and low in price. It is an ideal solid acid catalyst for increasing the content of 5-hydroxymethylfurfural released by pyrolysis of biomass, and shows great industrial application value.

[0066] The present invention also provides a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass, which is prepared by the above method for preparing a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass. Specifically, the zirconium oxide catalytic material has a loose porous structure formed by a combination of nano needles, wherein the nano needle structure has a thickness of 30-50 nm and a length of 200 nm-800 nm. The specific surface areas of the zirconium oxide solid acid catalysts prepared by the high-temperature carbonization-high-temperature calcination staged method and the direct calcination method are 65.61 m 2 / g and 38.38m 2 / g.

[0067] The present invention also provides a preparation device for a zirconium oxide catalytic material for pyrolyzing biomass to release 5-hydroxymethylfurfural, based on the main structure of an existing flat plate filter centrifuge, such as Figure 8 , Fig. 9 , Fig.10 As shown, the centrifuge body 1 includes a filter, the centrifuge body 1 includes an upper cover assembly, a body assembly, and a drum assembly. The body assembly includes a base 2, a casing 3 fixed on the base 2, a drum driving device 4 at the bottom of the casing 3, and a liquid outlet 5 at the bottom of the casing 3. The drum assembly includes a drum 6 arranged in the casing 3. The upper cover assembly includes an upper cover 7 hinged to the top of the casing 3, an observation mirror 8 at the top of the upper cover 7, and a feed pipe 9 at the top of the upper cover 7. When in use, the upper cover 7 is rotated to close, and the reaction liquid of the polytetrafluoroethylene reactor after the reaction is completed is fed into the drum 6 through the feed pipe 9. The liquid is discharged from the bottom of the feed pipe 9, and the drum 6 is driven to rotate at a high speed through the drum driving device 4. Meshes are evenly distributed on the side wall of the drum 6, and a filter membrane is also attached to the side wall of the drum 6. The reaction liquid rotating at a high speed in the drum 6 is centrifugally thrown out of the drum 6 through the filter membrane and the mesh, and the filtered water is discharged through the liquid outlet 5, leaving the precipitate obtained by centrifugation in the drum 6.

[0068] In particular, such as Figure 8 , Fig. 9 , Fig.10As shown, a movable ring net 10 is arranged around the inner side of the rotating drum 6, and a ring top plate 11 is arranged around the top of the movable ring net 10. The ring top plate 11 replaces the traditional material blocking ring plate at the top of the rotating drum 6. A movable lifting inner material pipe 12 is inserted into the feeding pipe 9. Specifically, a lifting cylinder can be arranged on one side of the feeding pipe 9 to drive the lifting movement of the inner material pipe 12. The inner material pipe 12 can also be designed as a multi-section telescopic structure. Conventional structures such as wire ropes are used. For example, a rotating drum for winding wire ropes is arranged on the upper cover 7, and the wire ropes can be moved upward and downward. One end of the rope is fixed to the bottom end of the inner material tube 12, and the lifting and lowering of the inner material tube 12 is controlled by driving the winding and unwinding of the wire rope. A horizontal stirring blade 13 is provided on the lower end side wall of the inner material tube 12, and a horizontal limiting blade 14 is provided on the upper end side wall of the inner material tube 12. The horizontal limiting blade 14 can be rotatably connected to the side wall of the inner material tube 12, and an elastic component such as a torsion spring is provided at the rotating connection. In the initial state, the horizontal limiting blade 14 pops out in a horizontal state. When the inner material tube 12 shrinks upward, the horizontal limiting blade 14 can be retracted downward into the side wall of the inner material tube 12;

[0069] The inner material pipe 12 moves upward until the top of the horizontal stirring blade 13 abuts against the annular top plate 11, driving the annular top plate 11 to move upward, and the movable ring net 10 moves upward close to the inner side of the drum 6, so that the mesh of the movable ring net 10 is opposite to the mesh of the drum 6, and the drum 6 rotates rapidly in a centrifugal mode;

[0070] The inner material pipe 12 moves downward until the horizontal stirring blade 13 extends into the bottom of the drum 6, and the bottom end of the horizontal limiting blade 14 abuts the annular top plate 11, driving the annular top plate 11 to move downward, and the movable ring net 10 moves downward close to the inner side of the drum 6, so that the mesh of the movable ring net 10 is misaligned with the mesh of the drum 6, that is, the mesh of the drum 6 is closed by the movable ring net 10, and the drum 6 rotates slowly in the washing mode, and the extended horizontal stirring blade 13 is stationary, which plays an auxiliary stirring and washing effect. Specifically, a washing pipe can be provided on the upper cover 7. In the washing mode, washing liquid is introduced into the drum 6 through the washing pipe, or the washing liquid can be directly introduced into the feeding pipe 9.

[0071] Among them, a vertical support rod is embedded and fixed on the movable ring network 10 in the vertical direction, and the top end of the vertical support rod is fixedly connected to the annular top plate 11 to play a supporting role. Preferably, the bottom end of the vertical support rod can also be inserted into a slot at the bottom end of the rotating drum 6, so that the movable ring network 10 as a whole can only move up and down, and cannot rotate circumferentially, which plays a further limiting support role.

[0072] In an embodiment of the present invention, Fig.11 , Fig.12 , Fig.13As shown, a through hole 15 is provided on one end of the annular top plate 11 close to the movable ring network 10, a movable block 16 is slidably connected inside the annular top plate 11, and an elastic member 17 is connected between the movable block 16. Specifically, the elastic member 17 can adopt existing elastic components such as springs, and the movable block 16 is pushed outward by the elastic member 17 so that one end of the movable block 16 closes the through hole 15. An upper limit block 18, a middle limit block 19 and a lower limit block 20 are fixed on the inner side wall of the rotating drum 6 from top to bottom. The end of the middle limit block 19 close to the rotating drum 6 is designed in a rectangular shape, and the upper and lower end surfaces of the middle limit block 19 away from the rotating drum 6 are designed in an inclined end surface. The upper and lower ends of the annular top plate 11 are elastically connected with movable rings 21 respectively. When the horizontal stirring blade 13 abuts against the annular top plate 11, the movable ring 21 at the lower end is pushed to drive the movable block 16 to slide inward and compress the elastic member. 17, at this time, the end of the movable block 16 slides to the inclined end surface of the lower end of the middle limit block 19, and as the horizontal stirring blade 13 continues to move upward, the annular top plate 11 is pushed, and the end of the movable block 16 is able to abut the inclined end surface of the lower end of the middle limit block 19, and continues to move inward and shrink horizontally until the movable block 16 moves to the inclined end surface of the upper end of the middle limit block 19, and the horizontal stirring blade 13 stops moving upward. At this time, although the horizontal stirring blade 13 no longer pushes up the annular top plate 11, the elastic member 17 pushes the movable block 16 outward, so that the movable block 16 slides along the inclined end surface of the upper end, driving the annular top plate 11 to move between the upper limit block 18 and the middle limit block 19, and the rotating drum 6 rotates rapidly in a centrifugal mode. The key point is that at this time, a gap is generated between the upward movement of the annular top plate 11 and the horizontal stirring blade 13, and the annular top plate 11 rotates with the rotating drum 6, and no friction interference is generated between the horizontal stirring blade 13;

[0073] When the transverse limiting leaf 14 abuts against the annular top plate 11, Fig.14 As shown, the movable ring 21 at the upper end is pushed to drive the movable block 16 to slide inward and compress the elastic member 17. At this time, the end of the movable block 16 slides to the inclined end surface of the upper end of the middle limit block 19. As the transverse limit leaf 14 continues to move downward to push the annular top plate 11, the end of the movable block 16 is able to abut the inclined end surface of the upper end of the middle limit block 19, and continues to move inward and contract, until the movable block 16 moves to the inclined end surface of the lower end of the middle limit block 19, as shown in FIG. Fig.15 As shown, the transverse limiting leaf 14 stops moving downward. At this time, although the transverse limiting leaf 14 no longer pushes down the annular top plate 11, the elastic member 17 pushes the movable block 16 outward, so that the movable block 16 slides along the inclined end surface of the lower end, as shown in FIG. Fig.16 As shown, the annular top plate 11 is driven to move between the lower limit block 20 and the middle limit block 19, and the drum 6 rotates slowly in the washing mode. The key point is that at this time, the annular top plate 11 moves downward and a gap is generated between the horizontal limit leaf 14. The annular top plate 11 rotates with the drum 6, and no friction interference is generated between the horizontal limit leaf 14;

[0074] The movable ring network 10 is provided with avoidance holes below the through-holes 15 for avoiding the upper limit block 18 , the middle limit block 19 and the lower limit block 20 .

[0075] In the embodiment of the present invention, a connecting rope 22 is connected between the movable block 16 and the movable ring 21. Specifically, Fig.13 As shown, one end of the movable block 16 is connected to the movable rings 21 at the upper and lower ends respectively by a connecting rope 22. The connecting rope 22 can adopt an existing conventional steel wire rope structure. The connecting rope 22 adopts a guide wheel structure conductor in the annular top plate 11. When the movable ring 21 is pressed inward, the movable block 16 is driven to move inward laterally through the connecting rope 22.

[0076] In an embodiment of the present invention, Figure 8 , Fig. 9 , Fig.10 As shown, the bottom end of the upper cover 7 is connected to an air inlet pipe 23 for spraying heating gas, such as hot air, toward the inside of the drum 6. The drum 6 rotates rapidly in a drying mode. A jacket can also be provided on the side wall of the housing 3. A heat-conducting medium is introduced into the jacket to conduct heat to the material in the drum 6 to assist in heating and drying or cooling. Thus, after the reaction liquid is generated in the polytetrafluoroethylene reactor, the reaction liquid is continuously centrifuged, washed, and dried. The obtained UiO-66 (Zr) powder is placed in a tubular furnace for calcination, and finally a porous zirconium oxide catalytic material ZrO2 is obtained.

[0077] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A method for preparing a zirconium oxide catalytic material for pyrolyzing biomass to release 5-hydroxymethylfurfural, characterized in that: The steps include: S1: preparing UiO-66 (Zr) sacrificial template agent, dissolving inorganic zirconium source and organic ligand powder in an acid mixture of N, N-dimethylformamide (DMF), stirring and ultrasonically treating the acid mixture until the inorganic zirconium source and organic ligand powder are completely dissolved and dispersed, adding the dissolved and dispersed mixed solution into a polytetrafluoroethylene reactor, reacting at 110°C to 150°C for 20 to 28 hours, and after the reaction, centrifuging or filtering the reaction product, washing the obtained precipitate with DMF and anhydrous ethanol for 3 times, respectively, drying and activating the washed precipitate, and finally obtaining UiO-66 (Zr) powder; S2 calcination is used to prepare zirconium oxide catalytic material. The selected UiO-66 (Zr) powder is placed in a tubular furnace and calcined in stages under nitrogen and air atmospheres, respectively. The calcination temperature is 500-800°C and the temperature is kept for 3-5 hours to obtain a porous zirconium oxide catalytic material ZrO2.

2. The method for preparing a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to claim 1, characterized in that: The selected inorganic zirconium source and organic ligand powder are ZrCl4 and terephthalic acid, the mass ratio of ZrCl4 and terephthalic acid is 1.2:1~1.5:1, the acid mixture includes N,N-dimethylformamide (DMF) and glacial acetic acid, the volume ratio of N,N-dimethylformamide and glacial acetic acid is 5:1~9:1, and the mixed solution after dissolution and dispersion is added into a polytetrafluoroethylene reactor for reaction.

3. The method for preparing a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to claim 1, characterized in that: The washed precipitate was dried at 100°C for 12 h, and then vacuum dried and activated at 150°C for 3 h to obtain UiO-66(Zr) white powder.

4. The method for preparing a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to claim 1, characterized in that: The obtained UiO-66 (Zr) powder was selected and placed in a tubular furnace. In a nitrogen atmosphere, the temperature was increased to 500-800°C at a heating rate of 5°C / min and calcined for 2 hours. Then, it was calcined in an air atmosphere and kept for 2 hours to obtain the zirconium oxide catalytic material ZrO2.

5. A zirconium oxide catalytic material for pyrolyzing biomass to release 5-hydroxymethylfurfural, wherein the zirconium oxide catalytic material is prepared by the method for preparing the zirconium oxide catalytic material for pyrolyzing biomass to release 5-hydroxymethylfurfural according to any one of claims 1 to 4.

6. The zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to claim 5, characterized in that: The zirconium oxide catalytic material has a loose porous structure formed by a combination of nano needles, wherein the thickness of the nano needle structure is 30-50nm, the length is 200nm-800nm, and the specific surface area is 35-70m 2 / g.

7. A preparation device for a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass, the preparation device being applied to the preparation method for a zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to any one of claims 1 to 4, comprising a filtering centrifuge body (1), the filtering centrifuge body (1) comprising an upper cover assembly, a body assembly, and a drum assembly, the body assembly comprising a base (2), a casing (3) fixed to the base (2), a drum driving device (4) at the bottom of the casing (3), and a liquid outlet (5) at the bottom of the casing (3), the drum assembly comprising a drum (6) arranged in the casing (3), the upper cover assembly comprising an upper cover (7) hinged to the top of the casing (3), an observation mirror (8) at the top of the upper cover (7), and a feed pipe (9) at the top of the upper cover (7), characterized in that: A movable ring net (10) is arranged around the inner side of the rotating drum (6), and an annular top plate (11) is arranged around the top of the movable ring net (10). A movable lifting inner material pipe (12) is inserted into the feeding pipe (9), and a horizontal stirring blade (13) is arranged on the lower side wall of the inner material pipe (12), and a horizontal limiting blade (14) is arranged on the upper side wall of the inner material pipe (12). The inner material pipe (12) moves upward until the top of the horizontal stirring blade (13) abuts against the annular top plate (11), thereby driving the annular top plate (11) to move upward, and the movable ring net (10) moves upward closely against the inner side of the rotating drum (6), so that the mesh of the movable ring net (10) is opposite to the mesh of the rotating drum (6), and the rotating drum (6) rotates rapidly in a centrifugal mode; The inner material tube (12) moves downward until the transverse stirring blade (13) extends into the bottom of the rotary drum (6), and the bottom end of the transverse limiting blade (14) abuts against the annular top plate (11), driving the annular top plate (11) to move downward, and the movable ring net (10) moves downward closely against the inner side of the rotary drum (6), so that the mesh of the movable ring net (10) is misaligned with the mesh of the rotary drum (6), and the rotary drum (6) rotates slowly in a washing mode.

8. The preparation device of zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to claim 7, characterized in that: A perforation (15) is provided on one end of the annular top plate (11) close to the movable ring network (10); a movable block (16) is slidably connected inside the annular top plate (11), and an elastic member (17) is connected between the movable block (16); the movable block (16) is pushed outward by the elastic member (17) so that one end of the movable block (16) closes the perforation (15); an upper limit block (18), a middle limit block (19) and a lower limit block (20) are fixed on the inner side wall of the rotating drum (6) in sequence from top to bottom; the middle limit block (19) is designed in a rectangular shape at one end close to the rotating drum (6); and the upper and lower end surfaces of the middle limit block (19) at one end away from the rotating drum (6) are designed in a rectangular shape. The inclined end surface is designed, and the upper and lower ends of the annular top plate (11) are elastically connected with movable rings (21). When the horizontal stirring blade (13) abuts against the annular top plate (11), it pushes the movable ring (21) at the lower end, drives the movable block (16) to slide inward, and compresses the elastic member (17) until the movable block (16) moves to the inclined end surface of the upper end of the middle limit block (19). The horizontal stirring blade (13) stops moving upward and pushes the movable block (16) through the elastic member (17) so that the movable block (16) slides along the inclined end surface of the upper end, drives the annular top plate (11) to move between the upper limit block (18) and the middle limit block (19), and the drum (6) rotates rapidly in a centrifugal mode; When the transverse limiting leaf (14) abuts against the annular top plate (11), it pushes the movable ring (21) at the upper end, drives the movable block (16) to slide inward, and compresses the elastic member (17) until the movable block (16) moves to the inclined end surface of the lower end of the middle limiting block (19), the transverse limiting leaf (14) stops moving downward, and pushes the movable block (16) through the elastic member (17) so that the movable block (16) slides along the inclined end surface of the lower end, drives the annular top plate (11) to move between the lower limiting block (20) and the middle limiting block (19), and the rotary drum (6) rotates slowly to enter a washing mode; The movable ring net (10) is provided with a clearance hole below the perforation (15) for evading an upper limit block (18), a middle limit block (19) and a lower limit block (20).

9. The preparation device of zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to claim 8, characterized in that: A connecting rope (22) is connected between the movable block (16) and the movable ring (21); when the movable ring (21) is pressed inward, the movable block (16) is driven to move inward laterally through the connecting rope (22).

10. The preparation device of zirconium oxide catalytic material for releasing 5-hydroxymethylfurfural by pyrolyzing biomass according to claim 7, characterized in that: The bottom end of the upper cover (7) is connected to an air inlet pipe (23) for spraying heated gas toward the inside of the drum (6), and the drum (6) rotates rapidly in a drying mode.

Citation Information

Patent Citations

  • Preparation and application methods of solid acid catalyst based on Zr-MOF

    CN108499579A

  • Preparation method and application of high-stability solid acid based on metal organic framework

    CN112742481A

  • CN (at) ZrO2 composite material and application thereof in catalysis of cycloaddition reaction of CO2 and epoxide

    CN114939431A

  • Preparation method of nano zirconium oxide with high specific surface area

    CN116020430A

  • MOFs-derived ordered mesoporous cerium-zirconium composite oxide as well as preparation method and application thereof

    CN116459823A

Cited By

  • Zirconium oxide loaded noble metal catalyst as well as preparation method and application thereof

    CN122164398A