Concrete modified by organic-inorganic composite internal curing agent

Through the use of organic-inorganic composite internal curing agent, combined with aminosilane coupling agent to modify inorganic nanoparticles and aramid nanofibers, the problem of shrinkage and cracking of concrete is solved, the mechanical properties and crack resistance of concrete are improved, and the structure is extended service life.

CN118702437BActive Publication Date: 2024-11-15SUZHOU CHUXIN MOYI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411195726.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-15
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Existing concrete internal curing agents are difficult to effectively prevent concrete from shrinking and cracking, resulting in reduced structural strength and shortened service life, especially the insufficient mechanical properties and crack resistance of high-strength concrete.

Method used

Using organic-inorganic composite internal curing agent, the inorganic nanoparticles are modified with aminosilane coupling agent and aramid nanofibers to form a hydrogel with high mechanical properties, enhancing the toughness and crack resistance of concrete, and passing through inorganic nanoparticles Improve dispersion performance and porosity.

Benefits of technology

It significantly improves the mechanical properties and crack resistance of concrete, reduces the gel water release shrinkage, enhances the flexural strength and crack resistance of concrete, and extends the service life of the structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118702437B_ABST
    Figure CN118702437B_ABST
Patent Text Reader

Abstract

The present invention relates to an organic-inorganic composite internal curing agent modified concrete, belonging to the technical field of concrete materials. The present invention uses aramid nanofibers as the base material of gel, which not only retains the advantages of traditional organic fiber materials, but also has significant characteristics such as high elastic modulus, hydrophilicity and surface activity, can effectively bridge the cracks generated at the matrix under the action of load, transfer the stress on the surface of the cracks, and transform the cement-based material from the original brittle failure to ductile failure, thereby enhancing and toughening the cement. The introduction of inorganic nanoparticles can not only prevent the aggregation and merging of aramid nanofiber bundles, but also disperse the stress on the gel, enhance the mechanical properties of the gel, reduce the water release shrinkage rate of the gel, and improve the mechanical properties and crack resistance of the concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an organic-inorganic composite internal curing agent modified concrete, belonging to the technical field of concrete materials. Background Art

[0002] Concrete has a long history of being used in engineering construction as the most widely used and largest-volume building material. Concrete was first made from lime and mortar through a simple mixing process, which is relatively simple compared to the more mature concrete technology currently available. The main components of concrete include two parts: one is the cementitious material and the other is the filling material. Concrete is widely used because its raw materials are easy to obtain and the cost is low. In addition, it also has the advantages of high plasticity and good fire resistance.

[0003] In view of the complex climate environment in various regions, such as temperature difference, dryness, strong wind, etc., the evaporation of water inside the concrete is accelerated, resulting in increased shrinkage and deformation of the concrete and increased risk of cracking, which poses great challenges and requirements for construction materials. Shrinkage cracking can cause a series of problems such as leakage, reduced strength, external erosion of the concrete structure, and even affect its service life in severe cases.

[0004] There are many reasons for concrete cracking, and inadequate maintenance is one of the important reasons. Adding curing agent is the main curing method for concrete. Most of the prior art uses super absorbent resin and nano cellulose gel as internal curing agent. For example, patents such as CN111892378A, CN 112321213A, and CN 116120018A all use nano cellulose as a gel frame for the mortar field. However, nano cellulose gel has poor mechanical properties and is difficult to meet the use requirements of high-strength concrete. It is mainly used in the field of thermal insulation mortar. Although CN116694126A prepares aramid nanofiber aerogel, it uses an in-situ polymerization process to prepare aramid nanofibers, and the fiber aspect ratio formed is small, the mechanical properties are poor, and the mechanical strength of the prepared aerogel is low, which can only be applied to the field of low-strength thermal insulation putty to achieve the technical effect of thermal insulation. Therefore, on the basis of preventing concrete cracking, improving the mechanical properties of concrete has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of the above problems, the main purpose of the present invention is to provide an organic-inorganic composite internal curing agent modified concrete.

[0006] The technical solution adopted by the present invention is:

[0007] An organic-inorganic composite internal curing agent modified concrete, wherein the mass ratio of cement to the organic-inorganic composite internal curing agent in the modified concrete is (600-650): (1-10);

[0008] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0009] (1) Modifying inorganic nanoparticles with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of the inorganic nanoparticles to the aminosilane coupling agent is 1:(0.1-1);

[0010] (2) placing aramid fibers into a reaction kettle containing alkali and dimethyl sulfoxide and stirring the mixture to prepare an aramid nanofiber dispersion;

[0011] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:(1-10);

[0012] (4) under stirring conditions, adding a protonated solvent dropwise to the mixed solution to obtain a hydrogel mixed solution by sol-gelation;

[0013] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0014] After the fresh concrete is poured, the volume of the concrete will decrease due to the hydration of the cementitious material and the changes in external moisture and temperature. This reduction in the volume of the concrete is called the shrinkage of the concrete. According to the causes of the shrinkage, the shrinkage of the concrete includes autogenous shrinkage, chemical shrinkage, drying shrinkage, etc. Internal curing is considered to be an effective curing method to reduce shrinkage. The prior art generally uses super absorbent resin as an internal curing material, but the super absorbent resin has a low porosity and poor fusion with components such as cement, and the holes generated after the resin releases water and shrinks can easily lead to a decrease in the compressive strength of the concrete. In previous work, the inventor used aramid nanofibers and inorganic fibers to composite to improve the performance of concrete. The composite fibers reduce the porosity of the concrete, increase the toughness of the concrete, and improve the performance of the concrete. However, the composite fibers cannot effectively inhibit the shrinkage of the concrete, resulting in the generation of fine cracks. In order to solve this problem, the present invention composites aramid nanofibers with inorganic nanoparticles to prepare an organic-inorganic composite aramid nanofiber gel as an internal curing agent.

[0015] Using aramid nanofibers as the base material of the gel, its mechanical properties are greatly enhanced compared to ordinary resin-type and nanocellulose-type gels. Aramid nanofibers not only retain the advantages of traditional organic fiber materials, but also have significant properties such as high elastic modulus, hydrophilicity and surface activity. They can effectively bridge the cracks generated in the matrix under load, transfer the stress on the crack surface, and transform the original brittle failure of cement-based materials into ductile failure, thus achieving the effect of strengthening and toughening.

[0016] However, the mechanical properties of pure aramid nanofiber gel are insufficient, and the shrinkage after water release is large. More importantly, although the aramid nanofiber prepared by the alkali / DMSO immersion method has a large aspect ratio and excellent mechanical properties, it is easy for the fiber bundles to merge in the aqueous solution, resulting in fiber agglomeration, which affects the porosity and water retention of the gel. Moreover, as an organic gel material, the aramid nanofiber gel will shrink in volume after water release, which seriously affects the safety, stability and durability of the structure. In order to improve the structural stability of the gel, the present invention first adds amino-modified inorganic nanoparticles to the mixed solution of alkali and dimethyl sulfoxide of aramid nanofibers, and then adds water; compared with first adding water to the aramid nanofiber dispersion and then adding amino-modified inorganic nanoparticles, the dispersion performance of the nanofibers can be more effectively improved. After modification by coupling agents, the inorganic nanoparticles will have active functional groups such as amino groups on their surfaces; the aramid nanofibers prepared by the alkaline solution method are electronegative and have a large number of reactive oxygen-containing functional groups such as carboxyl and hydroxyl groups, which can make the inorganic nanoparticles grafted onto the surface of the aramid nanofibers, thereby increasing the adhesion of the particles and improving the dispersion properties of the aramid nanofibers. The introduction of inorganic nanoparticles not only disperses the stress on the gel and enhances the mechanical properties of the gel, but also enhances the mechanical strength of the gel framework, reduces the shrinkage rate of the gel after water release, and improves the bending strength and crack resistance of the concrete.

[0017] Furthermore, in step (1), the aminosilane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-diethylenetriaminopropyltrimethoxysilane, 3-diethylenetriaminopropyltriethoxysilane, 3-diethylenetriaminopropylmethyldimethoxysilane, 3-diethylenetriaminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.

[0018] Furthermore, in step (1), the particle size of the inorganic nanoparticles is 50-500 nm.

[0019] Furthermore, the inorganic nanoparticles in step (1) are one or more of nano-silicon dioxide, nano-titanium dioxide, nano-zinc dioxide, and nano-calcium carbonate.

[0020] Furthermore, in step (1), the aminosilane coupling agent is one or more of 3-diethylenetriaminopropyltrimethoxysilane, 3-diethylenetriaminopropyltriethoxysilane, 3-diethylenetriaminopropylmethyldimethoxysilane, 3-diethylenetriaminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane. The above coupling agent is a polyaminosilane coupling agent. Compared with monoaminosilane coupling agents such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane, it has more active amino groups, which makes it easy for the inorganic nanoparticles to present positive charge, which is more conducive to the adsorption of inorganic nanoparticles. In particular, the aminosilane coupling agents in step (1) are 3-diethylenetriaminopropylmethyldimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane. Coupling agents with different chain lengths can give full play to the coupling modification effect of the coupling agents and improve the adhesion effect.

[0021] Furthermore, in step (2), the alkali is sodium hydroxide or potassium hydroxide; and the ratio of the aramid fiber, the alkali and the dimethyl sulfoxide is 1 g: (1-2) g: (350-500) mL.

[0022] Furthermore, the stirring in step (2) is carried out at room temperature for 3-8 days.

[0023] Furthermore, in step (4), the protonated solvent is one or more of formic acid, acetic acid, and hydrochloric acid.

[0024] Furthermore, the concrete comprises the following components by weight: 150-160 parts of water, 600-650 parts of cement, 100-110 parts of fly ash, 550-600 parts of sand, 800-850 parts of crushed stone, 1-10 parts of internal curing agent, 5-10 parts of water reducing agent, and 10-15 parts of expansion agent. The curing agent prepared by the present invention can be used for cement paste and modified concrete mixture, and can prevent shrinkage cracking during hydration and hardening.

[0025] The present invention has the following advantages: the aramid nanofiber is used as the basic material of the gel, which not only retains the advantages of traditional organic fiber materials, but also has significant characteristics such as high elastic modulus, hydrophilicity and surface activity, and can effectively bridge the cracks generated at the matrix under the load, transfer the stress on the crack surface, and transform the original brittle failure of the cement-based material into ductile failure, thereby achieving the effect of strengthening and toughening. The introduction of inorganic nanoparticles can not only prevent the aramid nanofiber bundles from agglomerating and merging, but also disperse the stress on the gel, enhance the mechanical properties of the gel, reduce the water release shrinkage rate of the gel, and improve the mechanical properties and crack resistance of the concrete. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a scanning electron microscope image of the internal curing agent prepared in Example 8;

[0027] Figure 2 This is a scanning electron microscope image of the internal curing agent prepared in Comparative Example 1;

[0028] Figure 3 This is a test chart of the water retention performance of the internal curing agent prepared in Examples 1-5;

[0029] Figure 4 This is a test chart of the water retention performance of the internal curing agent prepared in Examples 6-8 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Among them, the aramid fiber used in the embodiments of the present invention and the comparative example is DuPont Kevlar fiber.

[0031] Example 1

[0032] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 150 parts of water, 600 parts of sulphoaluminate cement, 100 parts of fly ash, 550 parts of sand, 800 parts of crushed stone, 4 parts of internal curing agent, 5 parts of polycarboxylate water reducer, and 10 parts of UEA expansion agent;

[0033] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0034] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.1; the aminosilane coupling agent is 3-diethylenetriaminepropylmethyldimethoxysilane; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0035] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 4 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g:1 g:350 mL;

[0036] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:1;

[0037] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0038] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0039] Example 2

[0040] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 160 parts of water, 650 parts of sulphoaluminate cement, 110 parts of fly ash, 600 parts of sand, 850 parts of crushed stone, 10 parts of internal curing agent, 10 parts of polycarboxylate water reducer, and 15 parts of UEA expansion agent;

[0041] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0042] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:1; the aminosilane coupling agent is N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0043] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, the alkali and the dimethyl sulfoxide is 1 g:2 g:500 mL;

[0044] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:10;

[0045] (4) under stirring conditions, adding protonated solvent acetic acid dropwise to the mixed solution to obtain a hydrogel mixed solution by sol-gelation;

[0046] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0047] Example 3

[0048] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 153 parts of water, 620 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 3 parts of internal curing agent, 6 parts of polycarboxylate water reducer, and 12 parts of UEA expansion agent;

[0049] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0050] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.3; the aminosilane coupling agent is N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0051] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 5 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, the alkali and the dimethyl sulfoxide is 1 g:1.2 g:400 mL;

[0052] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:3;

[0053] (4) under stirring conditions, adding a protonated solvent, hydrochloric acid, to the mixed solution to obtain a hydrogel mixed solution by sol-gelation;

[0054] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0055] Example 4

[0056] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 156 parts of water, 640 parts of sulphoaluminate cement, 108 parts of fly ash, 590 parts of sand, 840 parts of crushed stone, 8 parts of internal curing agent, 9 parts of polycarboxylate water reducer, and 13 parts of UEA expansion agent;

[0057] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0058] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.8; the aminosilane coupling agent is a mixture of N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane in a mass ratio of 1:1; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.6 h, filter and dry to obtain the modified inorganic nanoparticles;

[0059] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 5.5 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, the alkali and the dimethyl sulfoxide is 1 g:1.8 g:500 mL;

[0060] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:8;

[0061] (4) under stirring conditions, adding protonated solvent acetic acid dropwise to the mixed solution to obtain a hydrogel mixed solution by sol-gelation;

[0062] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0063] Example 5

[0064] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 155 parts of water, 630 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 5 parts of internal curing agent, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0065] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0066] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.6; the aminosilane coupling agent is 3-aminopropyltriethoxysilane; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0067] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g:1.4 g:420 mL;

[0068] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:5;

[0069] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0070] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0071] Example 6

[0072] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 155 parts of water, 630 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 5 parts of internal curing agent, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0073] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0074] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.6; the aminosilane coupling agent is 3-diethylenetriaminepropylmethyldimethoxysilane; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0075] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g:1.4 g:420 mL;

[0076] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:5;

[0077] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0078] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0079] Example 7

[0080] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 155 parts of water, 630 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 5 parts of internal curing agent, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0081] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0082] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.6; the aminosilane coupling agent is N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0083] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g:1.4 g:420 mL;

[0084] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:5;

[0085] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0086] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0087] Example 8

[0088] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 155 parts of water, 630 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 5 parts of internal curing agent, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0089] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0090] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.6; the aminosilane coupling agent is a mixture of 3-diethylenetriaminopropylmethyldimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane in a mass ratio of 1:1; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0091] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g:1.4 g:420 mL;

[0092] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:5;

[0093] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0094] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0095] Comparative Example 1

[0096] An organic internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 155 parts of water, 630 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 5 parts of internal curing agent, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0097] The preparation method of the organic internal curing agent comprises the following steps:

[0098] (1) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, the alkali and the dimethyl sulfoxide is 1 g:1.4 g:420 mL;

[0099] (2) adding deionized water to the aramid nanofiber dispersion and stirring to obtain a mixed solution;

[0100] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0101] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic internal curing agent.

[0102] Comparative Example 2

[0103] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 155 parts of water, 630 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 5 parts of internal curing agent, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0104] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0105] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.6; the aminosilane coupling agent is a mixture of 3-diethylenetriaminopropylmethyldimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane in a mass ratio of 1:1; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0106] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g:1.4 g:420 mL;

[0107] (3) adding deionized water to the aramid nanofiber dispersion, stirring evenly, and then adding modified inorganic nanoparticles to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:5;

[0108] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0109] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0110] Comparative Example 3

[0111] An organic-inorganic composite internal curing agent modified concrete, the concrete comprising the following components in parts by weight: 155 parts of water, 630 parts of sulphoaluminate cement, 106 parts of fly ash, 570 parts of sand, 820 parts of crushed stone, 15 parts of internal curing agent, 8 parts of polycarboxylate water reducer, and 14 parts of UEA expansion agent;

[0112] The preparation method of the organic-inorganic composite internal curing agent comprises the following steps:

[0113] (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of inorganic nanoparticles to aminosilane coupling agent is 1:0.6; the aminosilane coupling agent is a mixture of 3-diethylenetriaminopropylmethyldimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane in a mass ratio of 1:1; the inorganic nanoparticles are nano-calcium carbonate with a particle size of 200 nm; the specific modification process is to ultrasonically disperse the inorganic nanoparticles in a mixed solution of ethanol and deionized water in a volume ratio of 1:1, then add the aminosilane coupling agent to stir and react for 0.5 h, filter and dry to obtain the modified inorganic nanoparticles;

[0114] (2) placing aramid fiber in a reaction kettle containing alkali and dimethyl sulfoxide, and stirring at room temperature for 6 days to prepare an aramid nanofiber dispersion; the alkali is potassium hydroxide; and the ratio of the aramid fiber, alkali and dimethyl sulfoxide is 1 g:1.4 g:420 mL;

[0115] (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:5;

[0116] (4) under stirring conditions, adding a protonated solvent, formic acid, to the mixed solution to undergo sol-gelation to obtain a hydrogel mixed solution;

[0117] (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

[0118] The mechanical properties of concrete are tested according to GB / T 50081-2019; the cracking area of ​​concrete is tested according to GB / T 50082-2009.

[0119]

[0120] Figure 1 This is a scanning electron microscope image of the organic-inorganic composite internal curing agent prepared in Example 8; Figure 2 This is a scanning electron microscope image of the organic internal curing agent prepared in Comparative Example 1. It can be seen that Figure 1 Gel fiber compared Figure 2 Thinner, and Figure 1 The porosity and pore size of the curing agent are significantly better than Figure 2 This indicates that the introduction of inorganic nanoparticles promotes the dispersion of aramid nanofibers, prevents the fibers from merging, and enhances the mechanical properties. Figure 3-4This is a test diagram of the water retention performance of the internal curing agent prepared in Example 1-8 and Comparative Example 1-2. It can be seen from the figure that the introduction of inorganic nanoparticles not only promotes the dispersion of aramid nanofibers, but also increases the porosity, and the water retention performance is more excellent.

[0121] It can be seen from Examples 1-8 and Comparative Examples 1-3 that aramid nanofibers are used as the base material of the gel, which can effectively bridge the cracks generated at the matrix under the action of load, transfer the stress on the surface of the cracks, and play a role in strengthening and toughening. The introduction of inorganic nanoparticles not only disperses the stress on the gel and enhances the mechanical properties of the gel, but also plays a role in enhancing the mechanical strength of the gel framework, and reduces the water release shrinkage rate of the gel, thereby improving the bending strength and flexural strength of the concrete. It can be seen from Examples 5-8 that the polyaminosilane coupling agent has more active amino groups, which makes it easy for the inorganic nanoparticles to be positively charged, which is more conducive to the adsorption of inorganic nanoparticles. Example 8 shows that coupling agents of different chain lengths can give full play to the coupling modification effect of the coupling agent, improve the adhesion effect, and further improve the mechanical properties and water retention rate.

[0122] Compared with Example 8, Comparative Example 1 lacks only inorganic nanoparticles, and the porosity of the aramid nanofiber gel becomes smaller, agglomeration occurs, and the moisture retention performance becomes worse; and due to the lack of inorganic nanoparticles, the mechanical properties are reduced, and the water release shrinkage phenomenon is serious, which makes the concrete easy to crack. Compared with Example 8, Comparative Example 2 only has a different order of adding inorganic nanoparticles and deionized water. Deionized water is added to the aramid nanofiber dispersion first, which easily leads to fiber agglomeration and affects the performance of the curing agent. Compared with Example 8, Comparative Example 3 uses too much curing agent. Although it can prevent concrete from cracking, it leads to a decrease in its mechanical strength and cannot meet the use requirements of high-strength concrete.

[0123] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. An organic-inorganic composite internal curing agent modified concrete, It is characterized in that The mass ratio of cement and organic-inorganic composite internal curing agent in the modified concrete is (600-650): (1-10); The preparation method of the organic-inorganic composite internal curing agent comprises the following steps: (1) Inorganic nanoparticles are modified with an aminosilane coupling agent to obtain modified inorganic nanoparticles; the mass ratio of the inorganic nanoparticles to the aminosilane coupling agent is 1:(0.1-1); the aminosilane coupling agent is one or more of 3-diethylenetriaminopropyltrimethoxysilane, 3-diethylenetriaminopropyltriethoxysilane, 3-diethylenetriaminopropylmethyldimethoxysilane, 3-diethylenetriaminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane; (2) placing aramid fibers into a reaction kettle containing alkali and dimethyl sulfoxide and stirring the mixture to prepare an aramid nanofiber dispersion; (3) adding modified inorganic nanoparticles to the aramid nanofiber dispersion, stirring evenly, and then adding deionized water to obtain a mixed solution; wherein the mass ratio of the aramid fiber to the modified inorganic nanoparticles is 100:(1-10); (4) under stirring conditions, adding a protonated solvent dropwise to the mixed solution to obtain a hydrogel mixed solution by sol-gelation; (5) Solvent exchange is performed on the obtained hydrogel mixed solution and deionized water to obtain a hydrogel; the hydrogel is freeze-dried and crushed to obtain an organic-inorganic composite internal curing agent.

2. The organic-inorganic composite internal curing agent modified concrete according to claim 1, It is characterized in that The particle size of the inorganic nanoparticles in step (1) is 50-500 nm.

3. The organic-inorganic composite internal curing agent modified concrete according to claim 1, It is characterized in that The inorganic nanoparticles in step (1) are one or more of nano-silicon dioxide, nano-titanium dioxide, nano-zinc dioxide, and nano-calcium carbonate.

4. The organic-inorganic composite internal curing agent modified concrete according to claim 1, It is characterized in that In the step (1), the aminosilane coupling agents are 3-diethylenetriaminopropylmethyldimethoxysilane and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane.

5. The organic-inorganic composite internal curing agent modified concrete according to claim 1, It is characterized in that In the step (2), the alkali is sodium hydroxide or potassium hydroxide; and the ratio of the aramid fiber, the alkali and the dimethyl sulfoxide is 1 g: (1-2) g: (350-500) mL.

6. The organic-inorganic composite internal curing agent modified concrete according to claim 1, It is characterized in that The stirring in step (2) is performed at room temperature for 3-8 days.

7. The organic-inorganic composite internal curing agent modified concrete according to claim 1, It is characterized in that In the step (4), the protonated solvent is one or more of formic acid, acetic acid and hydrochloric acid.

8. The organic-inorganic composite internal curing agent modified concrete according to claim 1, Features: The concrete comprises the following components in parts by weight: 150-160 parts of water, 600-650 parts of cement, 100-110 parts of fly ash, 550-600 parts of sand, 800-850 parts of crushed stone, 1-10 parts of internal curing agent, 5-10 parts of water reducing agent and 10-15 parts of expansion agent.