A method for in-situ growth of B4C on SiC fiber
By growing the B4C coating in situ on SiC fibers, the problems of different interfacial uniformity and insufficient binding strength in chemical vapor deposition methods are solved, and the high binding strength and oxidation resistance are improved, avoiding the damage to the fibers by high-temperature heat treatment .
Patent Information
- Application Number
- CN202411179382.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing chemical vapor deposition methods for the preparation interface of SiC fiber surface have problems such as differences in interface uniformity, intimate coating bonding and damage to fibers by high-temperature heat treatment, resulting in insufficient mechanical properties and poor oxidation resistance.
Growing the B4C coating in situ on SiC fibers, ensuring the close bond between the B4C coating and SiC fibers by providing Si atomic vacancy and providing B4C interface growth under low air flow velocity environments, combined with H2 etching and stabilization treatment, ensures the close bond between the B4C coating and SiC fibers .
The bonding strength between the fiber and the coating is significantly improved, the coating decomposition and uniformity difference is avoided, the damage to the fibers is reduced by high-temperature treatment, and the mechanical properties and oxidation resistance of ceramic matrix composite materials are improved.
Smart Images

Figure CN118702497B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a ceramic-based composite material, and more particularly to a method for in-situ growing B4C on SiC fiber. Background Art
[0002] SiC / SiC composite is a high-performance ceramic-based composite material, and its basic structure consists of SiC fiber, interface phase and SiC matrix. In ceramic-based composite materials, the interface phase can play multiple roles, such as compensating for fiber surface defects, adjusting the physical and chemical compatibility between the matrix and the fiber reinforcement, transferring loads, and preventing the service environment from damaging the fiber. The current mainstream interface phases are boron nitride (BN), pyrolysis carbon (PyC) and their composite interface phases. The oxidation resistance of the PyC interface is poor, and it begins to oxidize at 500°C, generating gaseous oxides, which makes the interface phase lose its regulating function. The BN interface can repair fiber surface defects and deflect cracks, significantly improving the mechanical properties of ceramic-based composites, and its oxidation resistance is significantly better than that of PyC.
[0003] At present, the conventional method for preparing the interface on the surface of SiC fiber is: after the SiC fiber is solidified, chemical vapor deposition is carried out in a closed deposition furnace through a reaction atmosphere. In this chemical vapor deposition, first, the SiC fiber preform has a certain thickness. The different gas flow rates of the outer layer and the inner layer during interface deposition make the interface uniformity vary greatly, and it is easy for the outer layer deposition thickness to be significantly higher than the inner area. Secondly, the temperature of the coating prepared by chemical vapor deposition is low, and most of it is amorphous and easy to decompose. Further high-temperature heat treatment is required in other equipment to convert the amorphous into a crystalline state. During the transfer process, the coating is easy to decompose, which is not conducive to obtaining a highly crystalline coating. Finally, due to the limitations of the chemical vapor deposition (CVD) process, the fiber coating (BN and PyC) is not tightly bonded to the fiber matrix. Summary of the invention
[0004] In order to solve the above-mentioned problems caused by the chemical vapor deposition in the prior art to prepare the interface on the surface of SiC fiber, the present invention provides a method for in-situ growth of B4C on SiC fiber.
[0005] According to the method for in-situ growth of B4C on SiC fiber of the present invention, it comprises the following steps: S1, providing a SiC fiber preform; S2, placing the SiC fiber preform into a tubular furnace reaction chamber, evacuating the chamber and introducing an inert gas as a carrier gas, the pressure in the reaction chamber is 2 kPa-4 kPa, heating to 1100°C-1200°C and keeping the temperature for 0.5 h-1 h; S3, closing the carrier gas, introducing BCl3 into the reaction chamber to decompose it to release B, introducing H2 into the reaction chamber to etch the surface of the SiC fiber preform to provide Si atomic vacancies, reacting at 1 kPa-3 kPa, B filling the Si atomic vacancies to in-situ grow B4C, wherein the flow ratio of BCl3 to H2 is 1:(1-2); and S4, after the reaction is completed, the fiber preform is stabilized at 1100°C-1300°C for 10 min-30 min to obtain a SiC fiber with a B4C coating, and the bonding strength between the B4C coating and the SiC fiber is between 50 Between MPa and 75 MPa.
[0006] In one embodiment, the bonding strength between the B4C coating and the SiC fiber is 62.38 MPa. Compared with the bonding strength of conventional chemical vapor deposition of 30.24 MPa, the bonding strength between the fiber and the matrix of the present invention is significantly improved.
[0007] In a preferred embodiment, the SiC fiber preform is a SiC fiber bundle, a SiC fiber cloth, a SiC fiber two-dimensional stack, a SiC fiber two-dimensional stitched preform, a SiC fiber 3D braided preform, or a SiC fiber 2.5D braided preform.
[0008] In a preferred embodiment, step S1 includes degumming the SiC fiber preform. Specifically, the fixed SiC fiber preform is placed in a vacuum carbon tube furnace, and the degumming treatment is performed after vacuuming. The treatment temperature is 1100°C to 1300°C, and the vacuum insulation treatment in the furnace is 1h to 3h. In a preferred embodiment, the treatment temperature is 1200°C and the treatment time is 2h. It should be understood that the degumming treatment can remove the organic binder (commonly referred to as "glue") in the SiC fiber preform while avoiding damage to the fiber itself.
[0009] In a preferred embodiment, the inert gas is argon (Ar).
[0010] In a preferred embodiment, the vacuum degree of the vacuum state in step S2 is below 10 Pa. More preferably, the vacuum degree is below 5 Pa.
[0011] In a preferred embodiment, the heating rate of step S2 includes: the heating rate below 500°C is 9°C / min to 11°C / min, the heating rate between 500°C and 1000°C is 4°C / min to 6°C / min, and the heating rate above 1000°C is 2°C / min to 4°C / min. In a preferred embodiment, the heating rate of step S2 includes: the heating rate below 500°C is 10°C / min, the heating rate between 500°C and 1000°C is 5°C / min, and the heating rate above 1000°C is 3°C / min.
[0012] In a preferred embodiment, the reaction time of step S3 is 10 min to 30 min.
[0013] In a preferred embodiment, the stabilization treatment in step S4 is performed at a temperature of 1200° C. for 20 min.
[0014] In a preferred embodiment, the thickness of the B4C coating in step S4 is 10 nm to 200 nm.
[0015] According to the method for in-situ growth of B4C on SiC fiber of the present invention, Si atomic vacancies are provided by etching the surface of SiC fiber preform with H2, and the flow rate of H2 introduced is 1 to 2 times the flow rate of BCl3, so as to ensure that etching is carried out and sufficient vacancies are reserved, thereby in-situ growth of uniform B4C interface on the surface of SiC fiber, the residual carbon content inside the fiber is reduced and the bonding strength is improved, and the uniformity difference caused by the different flow rates of internal and external gases during deposition is avoided. The obtained B4C coating does not need to be transferred and is not easy to decompose, and is a highly crystalline coating. In summary, according to the method for in-situ growth of B4C on SiC fiber of the present invention, on the one hand, the bonding strength between the fiber and the coating is much higher than that of the traditional chemical vapor deposition method, and it is not easy to fall off in subsequent use. On the other hand, it avoids the damage to the fiber caused by the excessively high temperature (T>2000°C) of the traditional hot pressing sintering method. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The outer surface of the SiC fiber with in-situ grown B4C coating according to Example 1 of the present invention is shown by a SEM image.
[0017] Figure 2 yes Figure 1 Magnified image of .
[0018] Figure 3 The cross section of the SiC fiber with in-situ grown B4C coating according to Example 1 of the present invention is shown by a SEM image.
[0019] Figure 4 yes Figure 3 Magnified image of .
[0020] Figure 5 The outer surface of the SiC fiber according to Comparative Example 1 of the present invention is shown by a SEM image.
[0021] Figure 6 A cross section of the SiC fiber according to Comparative Example 1 of the present invention is shown by a SEM image. DETAILED DESCRIPTION
[0022] The preferred embodiments of the present invention are given below in conjunction with the accompanying drawings and described in detail.
[0023] Example 1
[0024] The SiC fiber bundle was fixed with a graphite clamp, placed in a vacuum carbon tube furnace, and then vacuumed for degumming treatment. The treatment temperature was 1100°C, and the vacuum insulation treatment was carried out in the furnace for 3 hours.
[0025] The degummed SiC fiber bundle was placed in the reaction chamber of a tubular furnace. After evacuation to a vacuum degree below 10 Pa, an inert gas was introduced as a carrier gas. The pressure in the reaction chamber was 2 kPa. The temperature was increased to 500 °C at a heating rate of 9 °C / min, then to 1000 °C at a heating rate of 4 °C / min, and then to 1100 °C at a heating rate of 2 °C / min and kept at this temperature for 1 h.
[0026] The carrier gas was turned off, and BCl3 and H2 were delivered to the reaction chamber through different gas inlet pipes, with a flow ratio of BCl3 and H2 of 1:1. B4C was grown in situ at 1 kPa for 30 min.
[0027] After the reaction, the fiber preform was stabilized at 1100 °C for 30 min to obtain SiC fiber with B4C coating. Figure 1-Figure 2 As shown, the surface of SiC fiber is layered with coating particles, such as Figure 3-Figure 4 As shown, the composition analysis shows that the surface in-situ reaction generates a B4C coating on the surface of the SiC fiber with a thickness of 126.9 nm.
[0028] Next, the bonding strength between the B4C coating and the SiC fiber of this embodiment is specifically characterized.
[0029] A metallographic mounting machine is used and filled with resin, which is cured at 120°C to 150°C to form a mounted sample containing a fiber-coating.
[0030] The thinning was carried out using a fully automatic inlay polishing machine with different polishing discs (400-5000 mesh), and double-sided mirror polishing was followed by ultrasonic-drying treatment.
[0031] The bonding strength between the fiber and the B4C coating was tested using a nanoindenter combined with a scanning electron microscope.
[0032] In this embodiment, the bonding strength between the B4C coating and the SiC fiber is 50 MPa.
[0033] Example 2
[0034] The SiC fiber cloth was fixed with a graphite clamp, placed in a vacuum carbon tube furnace, and then vacuumed for degumming treatment. The treatment temperature was 1200°C, and the vacuum insulation treatment was carried out in the furnace for 2 hours.
[0035] The degummed SiC fiber cloth was placed in the reaction chamber of a tubular furnace. After evacuation to a vacuum degree lower than 8 Pa, an inert gas was introduced as a carrier gas. The pressure in the reaction chamber was 3 kPa. The temperature was increased to 500°C at a heating rate of 10°C / min, then to 1000°C at a heating rate of 5°C / min, and then to 1150°C at a heating rate of 3°C / min and kept at this temperature for 45 min.
[0036] The carrier gas was turned off, and BCl3 and H2 were delivered to the reaction chamber through different gas inlet pipes, with a flow ratio of BCl3 and H2 of 1:1.5. B4C was grown in situ at 2 kPa for 20 min.
[0037] After the reaction, the fiber preform was stabilized at 1200°C for 20 min to obtain SiC fiber with B4C coating, wherein the bonding strength between the B4C coating and the SiC fiber was 62.38 MPa, and the thickness of the B4C coating was 150 nm.
[0038] Example 3
[0039] The two-dimensional stack of SiC fibers was fixed with a graphite fixture, placed in a vacuum carbon tube furnace, and evacuated to a vacuum degree below 10 Pa before degumming treatment. The treatment temperature was 1300°C, and the vacuum insulation treatment was performed in the furnace for 1 hour.
[0040] The degummed SiC fiber two-dimensional stack was placed in a tubular furnace reaction chamber. After evacuation, an inert gas was introduced as a carrier gas. The pressure in the reaction chamber was 4 kPa. The temperature was increased to 500°C at a heating rate of 11°C / min, then to 1000°C at a heating rate of 6°C / min, and then to 1200°C at a heating rate of 4°C / min and kept at this temperature for 0.5 h.
[0041] The carrier gas was turned off, and BCl3 and H2 were delivered to the reaction chamber through different gas inlet pipes, with a flow ratio of BCl3 and H2 of 1:2. B4C was grown in situ by reacting for 10 min at 3 kPa.
[0042] After the reaction, the fiber preform was stabilized at 1300°C for 10 min to obtain SiC fiber with B4C coating, wherein the bonding strength between the B4C coating and the SiC fiber was 75 MPa, and the thickness of the B4C coating was 200 nm.
[0043] Comparative Example 1
[0044] The SiC fiber bundle was fixed with a graphite clamp, placed in a vacuum carbon tube furnace, and then vacuumed for degumming treatment. The treatment temperature was 1100°C, and the vacuum insulation treatment was carried out in the furnace for 3 hours.
[0045] The degummed SiC fiber bundle was placed in the reaction chamber of a tubular furnace. After evacuation to a vacuum degree below 10 Pa, an inert gas was introduced as a carrier gas. The pressure in the reaction chamber was 2 kPa. The temperature was increased to 500 °C at a heating rate of 9 °C / min, then to 1000 °C at a heating rate of 4 °C / min, and then to 1100 °C at a heating rate of 2 °C / min and kept at this temperature for 1 h.
[0046] Turn off the carrier gas, and deliver BCl3 and H2 to the reaction chamber through different inlet pipes, respectively, and react at 4 kPa for 20 min. Figure 5-Figure 6 As shown, the surface of SiC fiber is smooth without obvious particle undulations.
[0047] Comparative Example 2
[0048] The B4C coating was deposited on the SiC fiber by chemical vapor deposition. The SiC fiber cloth was fixed with a graphite fixture, placed in a vacuum carbon tube furnace, and then vacuumed and debonded. The treatment temperature was 1200°C, and the vacuum insulation treatment was carried out in the furnace for 2 hours.
[0049] The degummed SiC fiber cloth was placed in the reaction chamber of a tubular furnace. After evacuation to a vacuum degree lower than 8 Pa, an inert gas was introduced as a carrier gas. The pressure in the reaction chamber was 3 kPa. The temperature was increased to 500°C at a heating rate of 10°C / min, then to 1000°C at a heating rate of 5°C / min, and then to 1100°C at a heating rate of 3°C / min and kept at this temperature for 45 min.
[0050] The carrier gas was turned off. In the first step, NH3, BCl3 and H2 were respectively delivered to the reaction chamber through different air inlet pipes, with a flow ratio of NH3, BCl3 and H2 of 1.2:1:0.5. The reaction was carried out at 1100°C for 30 minutes to generate an interface layer. In the second step, NH3, BCl3, H2 and phosgene were respectively delivered to the reaction chamber through different air inlet pipes, and the reaction was carried out at 1200°C for 30 minutes to allow the interface layer to adhere to the surface of the SiC fiber.
[0051] The heat treatment is performed at a temperature equal to or higher than 1500° C. for a duration of 4 hours.
[0052] In this comparative example, the bonding strength between the coating and the SiC fiber is 30.24 MPa.
[0053] The above is only a preferred embodiment of the present invention, and is not intended to limit the scope of the present invention. The above embodiment of the present invention can also be modified in various ways. That is, all simple, equivalent changes and modifications made according to the claims and the description of the present invention fall within the scope of protection of the claims of the present invention. The contents not described in detail in the present invention are all conventional technical contents.
Claims
1. A method for in-situ growth of B4C on SiC fiber, characterized in that: The method comprises the following steps: S1, providing a SiC fiber preform; S2, placing the SiC fiber preform into the reaction chamber of the tubular furnace, evacuating the chamber and passing an inert gas as a carrier gas, the pressure in the reaction chamber is 2 kPa~4 kPa, heating to 1100℃~1200℃ and keeping the temperature for 0.5 h~1 h; S3, closing the carrier gas, delivering BCl3 and H2 to the reaction chamber through different air inlet pipes, introducing BCl3 into the reaction chamber to decompose it and release B, introducing H2 into the reaction chamber to etch the surface of the SiC fiber preform to provide Si atomic vacancies, reacting at 1 kPa~3 kPa, B filling the Si atomic vacancies to in-situ grow B4C, wherein the flow ratio of BCl3 and H2 is 1:(1~2), and the reaction time is 10min~30min; and S4, after the reaction is completed, the fiber preform is stabilized at 1100℃~1300℃ for 10 min~30 min to obtain SiC fiber with B4C coating, and the bonding strength between the B4C coating and the SiC fiber is between 50 MPa~75 MPa.
2. The method according to claim 1, characterized in that The SiC fiber preform is a SiC fiber bundle, a SiC fiber cloth, a SiC fiber two-dimensional stack, a SiC fiber two-dimensional stitched preform, a SiC fiber 3D braided preform, or a SiC fiber 2.5D braided preform.
3. The method according to claim 1, characterized in that Step S1 includes debonding the SiC fiber preform.
4. The method according to claim 1, characterized in that: The inert gas is argon.
5. The method according to claim 1, characterized in that The heating rates of step S2 include: the heating rate below 500°C is 9°C / min~11°C / min, the heating rate between 500°C and 1000°C is 4°C / min~6°C / min, and the heating rate above 1000°C is 2°C / min~4°C / min.
6. The method according to claim 1, characterized in that The thickness of the B4C coating in step S4 is 10 nm to 200 nm.