Ultrasound-enhanced reversible deactivation free radical polymerization of vinylidene fluoride
Through the polymerization method of light and ultrasound coordinated regulation, the problem of difficult molecular structure in conventional polymerization methods is solved, and PVDF preparation with controllable molecular weight and narrow distribution is achieved at high conversion and high molecular weight, avoiding chain termination and transfer reactions. Improved catalytic efficiency.
Patent Information
- Application Number
- CN202411170554.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The conventional emulsion radical polymerization method of polyvinylidene fluoride is difficult to control due to chain termination and chain transfer reactions, and active chain aggregation under high conversion and high molecular weight conditions leads to irreversible reactions, making it difficult to achieve controllable molecular weight and molecular weight. Preparation of PVDF with narrow distribution.
Reversible inactivated radical polymerization method with coordinated regulation of light and ultrasound, using metal complexes as photocatalysts, water-soluble thioalkyl esterides as chain transfer agents and dimethyl carbonate as organic solvents, irradiation and ultrasound effects through light source , regulate polymerization reaction, reduce the aggregation and irreversible reaction of active chains.
PVDF preparation with controllable molecular weight and narrow molecular weight distribution under high conversion and high molecular weight conditions is achieved, avoiding chain termination and chain transfer reactions, and improving catalytic efficiency and product purity.
Smart Images

Figure CN118702850B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer compounds, and in particular relates to an ultrasound-enhanced reversible deactivated free radical polymerization method of vinylidene fluoride. Background Art
[0002] Polyvinylidene fluoride (PVDF) is widely used in coatings, lithium-ion batteries, water-oil separation, solar cells, water treatment and anti-corrosion materials due to its unique and excellent physical and chemical properties (oxidation resistance, high temperature resistance and chemical corrosion resistance, etc.), and ranks second in the use of fluorine-containing plastics. In industry, the common polymerization method of vinylidene fluoride is conventional emulsion free radical polymerization. For example, Chinese patent CN105085753A discloses a method for preparing polyvinylidene fluoride resin and its copolymer with high thermal stability, using perfluoropolyether carboxylate as emulsifier, peroxide as initiator, and water as continuous phase to prepare PVDF by polymerization at a certain temperature. However, conventional polymerization methods cannot accurately control the molecular structure of PVDF due to the existence of side reactions such as chain termination and chain transfer. The molecular weight of the obtained PVDF product is difficult to control and the molecular weight distribution is relatively wide.
[0003] Reversible addition-fragmentation chain transfer radical polymerization (RAFT) is one of the important means to precisely control the molecular structure of polymers. Bruno from France first used the RAFT method to synthesize fluorinated copolymers with a narrow molecular weight distribution in his research paper Macromolecules 2011, 44, 1841-1855, and proposed a new RAFT / MADIX method. On this basis, the research group further reported a light-controlled RAFT strategy (photoRAFT) in the research paper Macromolecules 2015, 48, 7810-7822, avoiding dead polymer chains caused by thermal decomposition of free radical initiators, and then synthesizing PVDF with controllable molecular weight and narrow molecular weight distribution.
[0004] However, the above two polymerization methods are only applicable to low conversion rate and low molecular weight conditions. The main reason is that there are two active chains in the polymerization system: PVDF-CH2-CF2· and PVDF-CF2-CH2·. As the polymerization conversion rate increases or the product molecular weight increases, the active chains in the polymerization system aggregate due to diffusion limitation due to poor compatibility, resulting in the more active PVDF-CH2-CF2· chains being prone to irreversible chain termination or chain transfer reactions, and the proportion of less active PVDF-CF2-CH2· chains gradually increasing. The reversible inactivation equilibrium process slows down, and the controllability of the product molecular structure becomes worse.
[0005] Conventional solutions to diffusion limitations (selecting a more compatible solvent or improving stirring efficiency) limit their application effectiveness due to the limited solubility of fluorinated monomers and polymers. Summary of the invention
[0006] The purpose of the present invention is to provide an ultrasound-enhanced reversible deactivated free radical polymerization method for polyvinylidene fluoride, which utilizes light and ultrasound to coordinately regulate the molecular weight and molecular weight distribution of polyvinylidene fluoride.
[0007] The ultrasound-enhanced reversible deactivation free radical polymerization method of polyvinylidene fluoride is as follows: after mixing a photocatalyst, a chain transfer agent and an organic solvent, polyvinylidene fluoride monomer is added, and polymerization reaction is carried out under light source irradiation and ultrasound conditions to obtain a reaction liquid, and the reaction liquid is post-treated to obtain polyvinylidene fluoride.
[0008] The photocatalyst is a metal complex, and the metal complex is tris[2-phenylpyridine-C2,N]iridium(III).
[0009] The chain transfer agent is a water-soluble thioalkyl ester.
[0010] The water-soluble thioalkyl ester is 2-ethoxythiosulfonylthiopropionic acid methyl ester.
[0011] The organic solvent is dimethyl carbonate.
[0012] The ratio of the vinylidene fluoride monomer, chain transfer agent, photocatalyst and organic solvent is 7-12:24-120:1-5:20-50, wherein the vinylidene fluoride monomer is measured in g, the chain transfer agent is measured in mg, the photocatalyst is measured in mg, and the organic solvent is measured in mL.
[0013] The light source is an LED light source with a wavelength range of 365-450nm.
[0014] The ultrasonic frequency is 20-80KHz.
[0015] The polymerization reaction temperature is room temperature, and the polymerization reaction time is 12-24 hours.
[0016] The post-treatment is purification, precipitation, centrifugation and drying in sequence.
[0017] The beneficial effects of the present invention are as follows:
[0018] (1) The present invention innovatively adds a water-soluble thioalkyl ester as a chain transfer agent, which can play a role in free radical exchange and buffering during the polymerization process, so that the number of growing chains is kept at a low level. The growth of the molecular chain is similar to the polymerization reaction probability of the monomer, so that the polymerization reaction exhibits the characteristics of active polymerization and improves the catalytic efficiency of the catalyst in the reaction system.
[0019] (2) In the present invention, light source irradiation can not only initiate polymerization reaction, but also alleviate the chain diffusion limitation in the PVDF polymerization system to a certain extent. However, the alleviation effect of light source irradiation is limited and cannot effectively avoid the aggregation of active chains in the polymerization system. Therefore, the present invention introduces ultrasound on the basis of light source irradiation, and strengthens the alleviation effect of light source irradiation through the mechanical waves generated by ultrasonic cavitation, thereby alleviating the chain diffusion limitation in the PVDF polymerization system from the molecular level under the action of elastic vibration.
[0020] (3) The present invention adopts light and ultrasound to coordinately regulate the ratio of the two active chains in the polymerization system, thereby reducing the influence of diffusion limitation of the polymer chains in the system due to poor compatibility, preventing the more active PVDF-CH2-CF2· from easily undergoing irreversible chain termination or chain transfer reactions, and realizing the preparation of PVDF with controllable molecular weight and narrow molecular weight distribution under high conversion rate and high molecular weight conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a diagram of the mechanism of light and ultrasound synergistically alleviating the diffusion limitation of polymer chains. The left figure is a diagram of the polymer chain state under light conditions, and the right figure is a diagram of the polymer chain state under light and ultrasound conditions.
[0022] Figure 2 The polyvinylidene fluoride obtained in Example 1 1 H NMR spectrum.
[0023] Figure 3 The polyvinylidene fluoride obtained in Example 1 19 F NMR spectrum.
[0024] Figure 4 This is the GPC spectrum of the polyvinylidene fluoride obtained in Example 1. DETAILED DESCRIPTION
[0025] The present invention is further described below with reference to the embodiments.
[0026] Example 1
[0027] 5 mg of tris[2-phenylpyridine-C2,N]iridium(III), 120 mg of methyl 2-ethoxythiothioylthiopropionate and 50 mL of dimethyl carbonate were added to a 100 ml reactor after being fully stirred and mixed. The oxygen in the mixture was removed by bubbling nitrogen and then vacuuming. 12 g of vinylidene fluoride monomer was added, and an LED visible light source with a wavelength of 450 nm and an ultrasonic transducer with a frequency of 80 KHz were turned on. The mixture was reacted at room temperature for 12 hours to obtain a reaction solution. The reaction solution was purified, precipitated, centrifuged and dried to obtain a polyvinylidene fluoride product. Polyvinylidene fluoride molecular weight measured by GPC M n=50040g / mol and the molecular weight distribution is M w / M n =1.18. The mechanism diagram of the synergistic effect of light and ultrasound on alleviating the diffusion limitation of polymer chains is shown in Figure 1 The product polyvinylidene fluoride 1 H NMR spectrum is shown in Figure 2 The peak at 2.73 ppm represents the hydrogen atoms in the polymer PVDF-CH2-CF2-R. 19 F NMR spectrum is shown in Figure 3 The peak at the negative shift of 92.39 ppm represents the fluorine atoms in the polymer PVDF-CH2-CF2-R. 1 H NMR spectra and 19 The F NMR spectrum can further verify that PVDF-CH2-CF2· is dominant in the polymerization system. The GPC spectrum of the product polyvinylidene fluoride is shown in Figure 4 .
[0028] Example 2
[0029] 3 mg of tris[2-phenylpyridine-C2,N]iridium(III), 24 mg of methyl 2-ethoxythiothioylthiopropionate and 30 mL of dimethyl carbonate were added to a 100 ml reactor after being fully stirred and mixed. The oxygen in the mixture was removed by bubbling nitrogen and then vacuuming. 10 g of vinylidene fluoride monomer was added, and an LED visible light source with a wavelength of 400 nm and an ultrasonic transducer with a frequency of 40 KHz were turned on. The mixture was reacted at room temperature for 16 hours to obtain a reaction solution. The reaction solution was purified, precipitated, centrifuged and dried to obtain a polyvinylidene fluoride product. Polyvinylidene fluoride molecular weight measured by GPC M n =84619 g / mol and the molecular weight distribution is M w / M n =1.30.
[0030] Example 3
[0031] 1 mg of tris[2-phenylpyridine-C2,N]iridium(III), 86 mg of methyl 2-ethoxythiothioylthiopropionate and 20 mL of dimethyl carbonate were added to a 100 ml reactor after being fully stirred and mixed. The oxygen in the mixture was removed by bubbling nitrogen and then vacuuming. 7 g of vinylidene fluoride monomer was added, and an LED visible light source with a wavelength of 365 nm and an ultrasonic transducer with a frequency of 20 KHz were turned on. The mixture was reacted at room temperature for 12 hours to obtain a reaction solution. The reaction solution was purified, precipitated, centrifuged and dried to obtain a polyvinylidene fluoride product. Polyvinylidene fluoride molecular weight measured by GPC Mn =57580g / mol and the molecular weight distribution is M w / M n =1.22.
[0032] Comparative Example 1
[0033] Without turning on ultrasound, the other steps were the same as in Example 1. Molecular weight of polyvinylidene fluoride measured by GPC M n =18268g / mol and the molecular weight distribution is M w / M n =1.71. Without the action of ultrasound, the molecular weight of the obtained polyvinylidene fluoride product is small and the molecular weight distribution is wide.
[0034] Comparative Example 2
[0035] Without turning on the light source, the other steps are the same as in Example 1. No polyvinylidene fluoride product is generated. In the absence of light source, no polymerization reaction occurs.
[0036] Comparative Example 3
[0037] The frequency was changed from 80 KHz to 200 KHz, and the other steps were the same as in Example 1. Molecular weight of polyvinylidene fluoride measured by GPC M n = 22971 g / mol and the molecular weight distribution is M w / M n =1.45. Due to the high-frequency ultrasonic degradation, the obtained polyvinylidene fluoride product has a small molecular weight and a wide molecular weight distribution.
Claims
1. A method for ultrasonically enhanced reversible deactivation free radical polymerization of vinylidene fluoride, characterized in that After the photocatalyst, chain transfer agent and organic solvent are mixed, vinylidene fluoride monomer is added, and a polymerization reaction is carried out under light source irradiation and ultrasonic conditions to obtain a reaction liquid, and the reaction liquid is post-treated to obtain polyvinylidene fluoride; the chain transfer agent is a water-soluble thioalkyl ester, and the ultrasonic frequency is 20-80KHz.
2. The ultrasound-enhanced reversible deactivation free radical polymerization method of vinylidene fluoride according to claim 1, characterized in that The photocatalyst is a metal complex.
3. The method for ultrasonically enhanced reversible deactivation free radical polymerization of vinylidene fluoride according to claim 2, characterized in that The metal complex is tris[2-phenylpyridine-C2,N]iridium(III).
4. The method for ultrasonically enhanced reversible deactivation free radical polymerization of vinylidene fluoride according to claim 1, characterized in that The water-soluble thioalkyl ester is methyl 2-ethoxythiothioylthiopropionate.
5. The method for ultrasonically enhanced reversible deactivation free radical polymerization of vinylidene fluoride according to claim 1, characterized in that The organic solvent is dimethyl carbonate.
6. The ultrasound-enhanced reversible deactivation free radical polymerization method of vinylidene fluoride according to claim 1, characterized in that The ratio of vinylidene fluoride monomer, chain transfer agent, photocatalyst and organic solvent is 7-12:24-120:1-5:20-50, wherein the vinylidene fluoride monomer is measured in g, the chain transfer agent is measured in mg, the photocatalyst is measured in mg, and the organic solvent is measured in mL.
7. The method for ultrasonically enhanced reversible deactivation free radical polymerization of vinylidene fluoride according to claim 1, characterized in that The light source is an LED light source with a wavelength range of 365-450nm.
8. The ultrasound-enhanced reversible deactivation free radical polymerization method of vinylidene fluoride according to claim 1, characterized in that The polymerization reaction temperature is room temperature, and the polymerization reaction time is 12-24 hours.
9. The ultrasound-enhanced reversible deactivation free radical polymerization method of vinylidene fluoride according to claim 1, characterized in that The post-processing is purification, precipitation, centrifugation and drying in sequence.