A highly flame-retardant and highly heat-insulating composite material for fire masks and a preparation method thereof

Through activation and chemical modification of kaolin, combined with vulcanization treatment of organic flame retardant and rubber and other materials, high flame retardant and strong heat insulation composite materials are prepared, which solves the problem of insufficient flame retardant and thermal insulation performance of fire mask materials, and realizes the Excellent flame retardant, thermal insulation and mechanical properties.

CN118703002BActive Publication Date: 2024-11-12GUANGZHOU YOUAN FIRE PROTECTION TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192742.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Fire mask materials have insufficient flame retardant and thermal insulation properties. The existing flame retardant produces smoke and toxic gases during combustion, and the thermal insulation effect is average.

Method used

The sodium hydroxide solution is used to activate kaolin, introduce alkenyl and carboxyl groups through ultrasonic dispersion and chemical reaction, combine with organic flame retardant to form flame retardant modified kaolin, and mix and vulcanize with brominated butyl rubber, silicone rubber and other materials to prepare High flame retardant and strong heat insulation composite material.

Benefits of technology

It significantly improves the flame retardant and thermal insulation properties of the material, reduces combustion speed and flame temperature, enhances mechanical properties and airtightness, and is suitable for high-performance protective materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of polymer materials, and discloses a highly flame-retardant and highly heat-insulating composite material for fire masks and a preparation method thereof. Bromobutyl rubber, silicone rubber, flame-retardant modified kaolin, antioxidant, lubricant, vulcanizing agent, magnesium oxide and zinc oxide are mixed, vulcanized and molded to obtain the highly flame-retardant and highly heat-insulating composite material for fire masks. The composite material can reduce the flame temperature and slow down the combustion speed, effectively preventing the transfer of heat, and has low thermal conductivity and excellent heat insulation effect. Kaolin and organic flame retardant act synergistically, have excellent flame retardancy, and have excellent chemical stability and mechanical properties. The composite material can effectively reduce the risk of injury to the wearer, is comfortable to wear, and is suitable for fire masks requiring high-performance protective materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a highly flame-retardant and highly heat-insulating composite material for fire masks and a preparation method thereof. Background Art

[0002] Fire masks are important personal protective equipment for firefighters at firefighting and rescue sites. They may face extreme environments such as high temperature, high smoke, and toxic gases. Therefore, strict requirements are placed on their performance. The materials used are preferably high-temperature resistant and highly flame-retardant and heat-insulating materials. They can protect firefighters from flames, high temperatures, and harmful gases under extreme conditions, ensuring the safety of firefighters’ lives. At the same time, they also need to ensure comfort and durability during use. The mask body of the fire mask is the skeleton that connects the various parts of the mask. It is usually made of highly elastic rubber material that is non-toxic and non-allergic to human skin. This material can fit various face shapes, provide good airtightness, and prevent toxic gases and smoke from entering the respiratory tract of escapees, but its flame retardant performance is poor.

[0003] Chinese patent application CN112341723A discloses a rubber material for a gas mask body with good flame retardancy and a preparation method thereof, the material comprises the following raw materials: rubber, reinforcing filler, vulcanizing agent, vulcanization accelerator, activator, antioxidant, softener and flame retardant, and provides a rubber material for a gas mask body with good flame retardancy and no elemental sulfur component, moderate hardness, high tensile stress, tensile strength and elongation at break, permanent deformation at break, low cold resistance coefficient, good flame retardancy and good anti-toxic performance, but the halogen flame retardant added in the material is easy to produce a large amount of smoke and toxic gas during the combustion process, which produces secondary harm to the human body, and the heat insulation performance is general. In recent years, with the continuous development of flame retardant technology, inorganic flame retardants and halogen-free flame retardants have been widely used in the field of fire protection due to their low smoke density, high oxygen index and excellent flame retardancy.

[0004] Therefore, developing a green, environmentally friendly, highly flame retardant and heat-insulating composite material is of great significance to improving the performance of fire masks. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In order to solve the above technical problems, the present invention provides a highly flame retardant and highly thermal insulating composite material for fire masks and a preparation method thereof, which solves the general problems of flame retardancy and thermal insulation properties of materials for fire masks.

[0007] (II) Technical solution

[0008] In order to achieve the above object, the present invention discloses a method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask, comprising the following steps:

[0009] Step 1, activating kaolin with sodium hydroxide solution, centrifuging and drying to obtain activated kaolin, adding the activated kaolin to a mixed solution of deionized water and anhydrous ethanol, ultrasonically dispersing, adding glacial acetic acid solution to adjust the pH, and then adding γ-methacryloxypropyltrimethoxysilane, stirring and mixing, reacting, cooling, centrifuging, washing, and drying in a vacuum drying oven at 60° C. for 24 hours to obtain olefinated kaolin;

[0010] Step 2, ultrasonically dispersing the olefinated kaolin in ethyl acetate, after uniform dispersion, adding itaconic acid and an initiator, stirring and mixing, reacting, cooling after the reaction, centrifuging, washing with ethyl acetate, and vacuum drying at 60° C. for 24 h to obtain carboxylated kaolin;

[0011] Step 3, ultrasonically dispersing the carboxylated kaolin in N,N-dimethylformamide, after uniform dispersion, adding 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine, mixing evenly, reacting, after the reaction is completed, filtering, washing with anhydrous ethanol, and vacuum drying at 60° C. for 12 h to obtain flame retardant modified kaolin;

[0012] Step 4: Evenly mix the brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant and lubricant, add them into an internal mixer for primary mixing, add vulcanizing agent, magnesium oxide and zinc oxide for secondary mixing, and obtain the rubber compound after the mixing is completed. After cooling, let it stand for 24 hours, transfer the rubber compound to a flat vulcanizer for vulcanization and molding to obtain a highly flame retardant and highly thermal insulating composite material for fire masks.

[0013] Preferably, the specific operation steps in step 1 are as follows: deionized water and sodium hydroxide are mixed evenly to obtain a sodium hydroxide solution, and then kaolin is added and mixed evenly, and the kaolin is activated and stirred at 90°C for 8 hours, wherein the mass ratio of deionized water, sodium hydroxide and kaolin is 100:0.3:5. After the activation treatment is completed, centrifugation is performed at a rate of 6000r / min for 8 minutes, and deionized water is used for washing, and vacuum drying is performed at 80°C for 48 hours to obtain activated kaolin, and the activated kaolin is added to a volume ratio of 1:8 of deionized water and anhydrous To the mixed solution of ethanol, glacial acetic acid solution is added to adjust the pH to 5, ultrasonic dispersion is carried out for 1 hour, γ-methacryloxypropyltrimethoxysilane is added, stirred and mixed, and a reaction occurs, wherein the mass ratio of the mixed solution, the activated kaolin, and γ-methacryloxypropyltrimethoxysilane is 900:100:25, the reaction temperature is 85°C, and the reaction time is 6 hours. After the reaction is completed, the mixture is cooled and centrifuged at a rate of 6000 r / min and a centrifugation time of 8 minutes. The mixture is washed with anhydrous ethanol and dried in a vacuum drying oven at 60°C for 24 hours to obtain olefinated kaolin.

[0014] Preferably, in the step 2, the mass ratio of olefinated kaolin, ethyl acetate, itaconic acid and initiator is 100:1500-1800:72-90:1-3.

[0015] Preferably, the reaction temperature in step 2 is 75-85° C., and the reaction time is 5-8 h.

[0016] Preferably, the initiator in step 2 is dibenzoyl peroxide.

[0017] Preferably, in the step three, the mass ratio of carboxylated kaolin, N,N-dimethylformamide, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole, and triethylamine is 100:2500-3500:142-160:21-34:12-15:70-120.

[0018] Preferably, the reaction temperature in step 3 is 30-35° C., and the reaction time is 8-10 h.

[0019] Preferably, in step 4, the mass ratio of brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant, lubricant, vulcanizing agent, magnesium oxide and zinc oxide is 100:25-40:4-9:0.5-1:1.2-2:1.5-3:0.5-1.2:0.8-1.5.

[0020] Preferably, in step 4, one or more of antioxidant 168, antioxidant 1010 and p-aminodiphenylamine are used.

[0021] Preferably, the lubricant in step 4 comprises one or more of polyethylene wax, calcium stearate and stearic acid.

[0022] Preferably, in step 4, the vulcanizing agent consists of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:2.

[0023] Preferably, in step 4, the temperature of the first mixing is 75-85° C., the time of the first mixing is 30-35 min, the temperature of the second mixing is 100-120° C., and the time of the second mixing is 20-30 min.

[0024] Preferably, the vulcanization temperature in step 4 is 170-180° C., and the vulcanization time is 10-18 min.

[0025] A highly flame retardant and highly heat-insulating composite material for firefighting masks is prepared by adopting the method for preparing the highly flame retardant and highly heat-insulating composite material for firefighting masks.

[0026] 3. Beneficial technical effects

[0027] (1) In the present invention, kaolin is first activated with sodium hydroxide solution, and the activated kaolin reacts with γ-methacryloxypropyltrimethoxysilane to introduce alkenyl groups on the surface of kaolin to obtain alkenylated kaolin. The alkenylated kaolin and itaconic acid undergo in-situ polymerization under the action of an initiator to introduce carboxyl groups on kaolin to obtain carboxylated kaolin. The carboxylated kaolin and the amino groups on 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide undergo amidation reaction to introduce an organic flame retardant to obtain flame retardant modified kaolin. Bromobutyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant, lubricant, vulcanizer, magnesium oxide and zinc oxide are mixed, vulcanized and molded to obtain a highly flame retardant and highly heat-insulating composite material for fire masks.

[0028] (2) Kaolin in the present invention is a natural mineral resource that meets the requirements of sustainable development. Kaolin has a layered structure and low thermal conductivity, which can effectively prevent the transfer of heat, thereby achieving a heat-insulating effect. During the combustion of the matrix, kaolin releases a large amount of water vapor and carbon dioxide, which can effectively dilute the oxygen concentration in the combustion area, reduce the flame temperature, and slow down the combustion rate. At the same time, water vapor can also absorb a large amount of heat, further reducing the temperature in the combustion area. Modification of kaolin effectively avoids the agglomeration of kaolin and can be evenly dispersed in the matrix. The introduced itaconic acid can not only improve the dispersibility of kaolin, but also significantly improve the flame retardancy of the matrix. At the same time, after itaconic acid is combined with kaolin and added to the composite material, it may change the pyrolysis behavior of the material, reduce the heat released by the material during combustion, thereby reducing the combustion rate and improving the self-extinguishing property of the material. Furthermore, after copolymerization of itaconic acid and kaolin, the mechanical properties of the matrix can be effectively improved, and while maintaining flame retardant properties, it also has high mechanical properties such as strength and toughness. An organic flame retardant containing phosphorus heterocycles and amino groups is introduced into kaolin. During the combustion of the matrix, the phosphorus heterocycles will generate acidic substances such as phosphoric acid and phosphorous acid, which promote the carbonization of the matrix and prevent the combustion reaction. The PO· free radicals generated during the combustion process can capture the ·OH and H· free radicals in the flame, interrupt the combustion chain reaction, and reduce the heat released by the combustion. At the same time, a large amount of nitrogen-containing non-combustible gas will be generated, which effectively dilutes the concentration of oxygen in the combustion system and further improves the flame retardant effect. The silicon element introduced during the reaction can further increase the density of the carbon layer. The synergistic effect of kaolin and organic flame retardants can prepare a composite material with excellent flame retardant properties.

[0029] (3) The brominated butyl rubber used in the present invention has good flame retardant properties, can significantly slow down the burning rate of the material, reduce the risk of fire, and has excellent air tightness, good bonding performance, fast vulcanization speed, and good compatibility with silicone rubber. The prepared composite material can maintain structural stability and durability. Silicone rubber has excellent high temperature resistance, can maintain stable physical and chemical properties under high temperature environment, and has strong aging resistance, can maintain the performance of the material unchanged for a long time, and extend the service life of the fire mask. Furthermore, silicone rubber has good softness and elasticity, can fit the facial contour closely, and improve wearing comfort and sealing. The highly flame retardant and strong heat-insulating composite material has excellent flame retardancy, heat insulation, chemical stability and mechanical properties, can effectively reduce the risk of injury to the wearer, and is suitable for fire masks that require high-performance protective materials. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] Example 1, (1) Ultrasonic dispersion of olefinic kaolin in ethyl acetate, after uniform dispersion, adding itaconic acid and initiator dibenzoyl peroxide, stirring and mixing, wherein the mass ratio of olefinic kaolin, ethyl acetate, itaconic acid and initiator is 100:1500:72:1, reacting at 75°C for 8 hours, after the reaction is completed, cooling, centrifuging, washing with ethyl acetate, and vacuum drying at 60°C for 24 hours to obtain carboxylated kaolin;

[0032] (2) Ultrasonic dispersion of carboxylated kaolin in N,N-dimethylformamide, after uniform dispersion, add 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine, and mix well. The carboxylated kaolin, N,N-dimethylformamide, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine. The mass ratio of -3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole, and triethylamine is 100:2500:142:21:12:70, and the reaction is carried out at 30°C for 10 hours. After the reaction is completed, the mixture is filtered, washed with anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain flame-retardant modified kaolin;

[0033] (3) The brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant and lubricant are mixed evenly and added into an internal mixer for mixing once. The mixing temperature is 75°C and the mixing time is 35 min. After mixing, vulcanizing agent, magnesium oxide and zinc oxide are added. The mass ratio of brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant 1010, lubricant polyethylene wax, vulcanizing agent, magnesium oxide and zinc oxide is 100:25:4:0.5:1.2. :1.5:0.5:0.8, the vulcanizing agent is composed of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:2, and secondary mixing is carried out. The temperature of the secondary mixing is 100°C, and the time of the secondary mixing is 30 minutes. After the mixing is completed, the rubber compound is obtained. After cooling, it is allowed to stand for 24 hours. The rubber compound is transferred to a flat vulcanizer for vulcanization and molding. The vulcanization temperature is 170°C, and the vulcanization time is 18 minutes to obtain a highly flame retardant and highly thermal insulating composite material for fire masks.

[0034] Example 2, (1) Ultrasonic dispersion of olefinic kaolin in ethyl acetate, after uniform dispersion, adding itaconic acid and initiator dibenzoyl peroxide, stirring and mixing, wherein the mass ratio of olefinic kaolin, ethyl acetate, itaconic acid, and initiator is 100:1700:82:2.1, reacting at 80°C for 6 hours, cooling after the reaction, centrifuging, washing with ethyl acetate, and vacuum drying at 60°C for 24 hours to obtain carboxylated kaolin;

[0035] (2) Ultrasonic dispersion of carboxylated kaolin in N,N-dimethylformamide, after uniform dispersion, add 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine, and mix well. The carboxylated kaolin, N,N-dimethylformamide, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine. The mass ratio of -3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole, and triethylamine is 100:3200:152:28:14:105, and the reaction is carried out at 32°C for 9 hours. After the reaction is completed, the mixture is filtered, washed with anhydrous ethanol, and vacuum dried at 60°C for 12 hours to obtain flame-retardant modified kaolin;

[0036] (3) The brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant and lubricant are mixed evenly and added into an internal mixer for mixing once. The mixing temperature is 80°C and the mixing time is 32 minutes. After mixing, vulcanizing agent, magnesium oxide and zinc oxide are added. The mass ratio of brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant 1010, lubricant polyethylene wax, vulcanizing agent, magnesium oxide and zinc oxide is 100:30:6:0.6:1. .5:2:0.8:1, the vulcanizing agent is composed of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:2, and secondary mixing is carried out. The temperature of the secondary mixing is 110°C, and the time of the secondary mixing is 25 minutes. After the mixing is completed, the rubber compound is obtained. After cooling, it is allowed to stand for 24 hours. The rubber compound is transferred to a flat vulcanizer for vulcanization and molding. The vulcanization temperature is 175°C, and the vulcanization time is 15 minutes to obtain a highly flame retardant and highly thermal insulating composite material for fire masks.

[0037] Example 3, (1) Bromobutyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant and lubricant are mixed uniformly, added into an internal mixer for primary mixing, the primary mixing temperature is 80°C, the primary mixing time is 34 min, after mixing, vulcanizing agent, magnesium oxide and zinc oxide are added, wherein the mass ratio of bromobutyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant 1010, lubricant polyethylene wax, vulcanizing agent, magnesium oxide and zinc oxide is 100:35:8:0.8: 1.8:2.5:1:1.2, the vulcanizing agent is composed of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:2, and secondary mixing is carried out. The temperature of the secondary mixing is 115°C and the time of the secondary mixing is 28 minutes. After the mixing is completed, the rubber compound is obtained. After cooling, it is allowed to stand for 24 hours. The rubber compound is transferred to a flat vulcanizer for vulcanization and molding. The vulcanization temperature is 175°C and the vulcanization time is 16 minutes to obtain a highly flame retardant and highly thermal insulating composite material for fire masks.

[0038] The preparation method of the flame retardant modified kaolin is the same as the preparation method of the flame retardant modified kaolin in Example 2.

[0039] Example 4, (1) ultrasonically disperse olefinic kaolin in ethyl acetate, after uniform dispersion, add itaconic acid and initiator dibenzoyl peroxide, stir and mix, wherein the mass ratio of olefinic kaolin, ethyl acetate, itaconic acid and initiator is 100:1800:90:3, react at 85°C for 5 hours, after the reaction is completed, cool, centrifuge, wash with ethyl acetate, and vacuum dry at 60°C for 24 hours to obtain carboxylated kaolin; (2) ultrasonically disperse carboxylated kaolin in N,N-dimethylformamide, after uniform dispersion, add 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide , 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine, mixed evenly, wherein the mass ratio of carboxylated kaolin, N,N-dimethylformamide, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine is 100:3500:160:34:15:120, react at 35°C for 8 hours, after the reaction is completed, filter, wash with anhydrous ethanol, and vacuum dry at 60°C for 12 hours to obtain flame retardant modified kaolin;

[0040] (3) The brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant and lubricant are mixed evenly and added into an internal mixer for a mixing process. The mixing temperature is 85°C and the mixing time is 30 min. After mixing, vulcanizing agent, magnesium oxide and zinc oxide are added. The mass ratio of brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant 1010, lubricant polyethylene wax, vulcanizing agent, magnesium oxide and zinc oxide is 100:40:9:1:2: 3:1.2:1.5, the vulcanizing agent is composed of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:2, and secondary mixing is carried out. The secondary mixing temperature is 120°C and the secondary mixing time is 20 minutes. After mixing, the rubber compound is obtained. After cooling, it is allowed to stand for 24 hours. The rubber compound is transferred to a flat vulcanizer for vulcanization and molding. The vulcanization temperature is 180°C and the vulcanization time is 10 minutes to obtain a highly flame retardant and highly thermal insulating composite material for fire masks.

[0041] Comparative Example 1, (1) Ultrasonic dispersion of olefinic kaolin in ethyl acetate, after uniform dispersion, adding itaconic acid and initiator dibenzoyl peroxide, stirring and mixing, wherein the mass ratio of olefinic kaolin, ethyl acetate, itaconic acid, and initiator is 100:1700:82:2.1, reacting at 80°C for 6 hours, cooling after the reaction, centrifuging, washing with ethyl acetate, and vacuum drying at 60°C for 24 hours to obtain carboxylated kaolin;

[0042] (2) The bromobutyl rubber, silicone rubber, carboxylated kaolin, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, antioxidant and lubricant were mixed evenly and added into an internal mixer for mixing once. The mixing temperature was 80°C and the mixing time was 34 min. After mixing, a vulcanizing agent, magnesium oxide and zinc oxide were added. The bromobutyl rubber, silicone rubber, carboxylated kaolin, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, antioxidant 1 010. The mass ratio of lubricant polyethylene wax, vulcanizing agent, magnesium oxide and zinc oxide is 100:35:3.2:4.8:0.8:1.8:2.5:1:1.2. The vulcanizing agent is composed of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:2. Secondary mixing is carried out. The temperature of the secondary mixing is 115°C and the time of the secondary mixing is 28 minutes. After the mixing is completed, the rubber compound is obtained. After cooling, it is allowed to stand for 24 hours. The rubber compound is transferred to a flat vulcanizer for vulcanization and molding. The vulcanization temperature is 175°C and the vulcanization time is 16 minutes to obtain a highly flame retardant and highly thermally insulating composite material for fire masks.

[0043] Comparative Example 2, (1) bromobutyl rubber, silicone rubber, kaolin, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, antioxidant and lubricant were mixed uniformly, added into an internal mixer for mixing once, the mixing temperature was 80°C, the mixing time was 34 min, after mixing, vulcanizing agent, magnesium oxide and zinc oxide were added, wherein bromobutyl rubber, silicone rubber, kaolin, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, antioxidant 10 10. The mass ratio of lubricant polyethylene wax, vulcanizing agent, magnesium oxide and zinc oxide is 100:35:3.2:4.8:0.8:1.8:2.5:1:1.2. The vulcanizing agent is composed of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:2. Secondary mixing is carried out. The temperature of the secondary mixing is 115°C and the time of the secondary mixing is 28 minutes. After the mixing is completed, the rubber compound is obtained. After cooling, it is allowed to stand for 24 hours. The rubber compound is transferred to a flat vulcanizer for vulcanization and molding. The vulcanization temperature is 175°C and the vulcanization time is 16 minutes to obtain a highly flame retardant and highly thermally insulating composite material for fire masks.

[0044] The preparation method of olefinated kaolin in the embodiment and the comparative example is as follows: deionized water and sodium hydroxide are mixed evenly to obtain a sodium hydroxide solution, and then kaolin is added and mixed evenly, and the kaolin is activated and stirred at 90° C. for 8 h, wherein the mass ratio of deionized water, sodium hydroxide and kaolin is 100:0.3:5. After the activation treatment is completed, centrifugation is performed at a rate of 6000 r / min for 8 min, and deionized water is used for washing, and vacuum drying is performed at 80° C. for 48 h to obtain activated kaolin, and the activated kaolin is added to deionized water with a volume ratio of 1:8. and anhydrous ethanol, add glacial acetic acid solution to adjust the pH to 5, ultrasonically disperse for 1 hour, add γ-methacryloxypropyltrimethoxysilane, stir and mix to react, wherein the mass ratio of the mixed solution, the activated kaolin and γ-methacryloxypropyltrimethoxysilane is 900:100:25, the reaction temperature is 85°C, and the reaction time is 6 hours. After the reaction is completed, cool and centrifuge at a rate of 6000 r / min and a centrifugation time of 8 minutes, wash with anhydrous ethanol, and dry in a vacuum drying oven at 60°C for 24 hours to obtain olefinated kaolin.

[0045] The kaolin used in the examples and comparative examples of the present invention was purchased from Shangxing Chemical Co., Ltd., Dianbai District, Maoming City; the CAS number of 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide is 18695-58-4, and the molecular formula is ; Bromobutyl rubber was purchased from ExxonMobil Corporation of the United States, model number Bromobutyl 2244; silicone rubber was methyl vinyl silicone rubber purchased from Zhonghao Chenguang Chemical Research Institute Co., Ltd., brand number 110-2; other undisclosed reagents were commercially available.

[0046] The composite materials prepared in Examples 1-4 and Comparative Examples 1-2 were subjected to corresponding tests, and the test methods and test results are as follows:

[0047] (1) Flame retardant performance test: The composite material was cut into square specimens and subjected to limiting oxygen index test on JF-5 oxygen index analyzer. Each group was tested three times and the average value was taken. The composite material was subjected to cone calorimetry test according to ISO5660 standard and tested on American Motis CCT cone calorimeter.

[0048] (2) Thermal insulation performance test: Thermal conductivity test was conducted according to GB / T 11205-2009 standard, using the QTM500 thermal conductivity tester produced by Hitachi Ltd. of Japan;

[0049] The above test results are shown in Table 1:

[0050] Table 1 Relevant performance test table of the composite materials in Examples 1-4 and Comparative Examples 1-2

[0051]

[0052] According to the test results in Table 1, it can be seen that the composite materials corresponding to Examples 1-4 have excellent flame retardant properties, and the corresponding limiting oxygen indexes all reach the flame retardant level. In Comparative Example 1, carboxylated kaolin and organic flame retardant were directly added, the dispersibility was reduced, the compatibility with the matrix deteriorated, and the flame retardant performance was reduced. In Comparative Example 2, kaolin was not modified, and the limiting oxygen index of the corresponding composite material was 26.8%, which failed to pass the UL-94 test. The corresponding thermal conductivity of Examples 1-4 is low, and the thermal insulation performance is excellent, among which the corresponding thermal conductivity of Example 3 is , good thermal insulation performance.

[0053] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask, characterized in that: The steps include: Step 1, activating kaolin with sodium hydroxide solution, centrifuging and drying to obtain activated kaolin, adding the activated kaolin to a mixed solution of deionized water and anhydrous ethanol, ultrasonically dispersing, adding glacial acetic acid solution to adjust the pH, and then adding γ-methacryloxypropyltrimethoxysilane, stirring and mixing, reacting, cooling, centrifuging, washing, and drying in a vacuum drying oven at 60° C. for 24 hours to obtain olefinated kaolin; Step 2, ultrasonically dispersing the olefinated kaolin in ethyl acetate, after uniform dispersion, adding itaconic acid and an initiator, stirring and mixing, reacting, cooling after the reaction, centrifuging, washing with ethyl acetate, and vacuum drying at 60° C. for 24 h to obtain carboxylated kaolin; Step 3, ultrasonically dispersing the carboxylated kaolin in N,N-dimethylformamide, after uniform dispersion, adding 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole and triethylamine, mixing evenly, reacting, after the reaction is completed, filtering, washing with anhydrous ethanol, and vacuum drying at 60° C. for 12 h to obtain flame retardant modified kaolin; Step 4: Evenly mix the brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant and lubricant, add them into an internal mixer for primary mixing, add vulcanizing agent, magnesium oxide and zinc oxide for secondary mixing, and obtain the rubber compound after the mixing is completed. After cooling, let it stand for 24 hours, transfer the rubber compound to a flat vulcanizer for vulcanization and molding to obtain a highly flame retardant and highly thermal insulating composite material for fire masks.

2. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: The specific operation steps in step 1 are as follows: deionized water and sodium hydroxide are mixed evenly to obtain a sodium hydroxide solution, and then kaolin is added and mixed evenly, and the kaolin is activated and stirred at 90° C. for 8 hours, wherein the mass ratio of deionized water, sodium hydroxide and kaolin is 100:0.3:

5. After the activation treatment is completed, centrifugation is performed at a rate of 6000 r / min for 8 minutes, and deionized water is used for washing, and vacuum drying is performed at 80° C. for 48 hours to obtain activated kaolin, and the activated kaolin is added to a solution of deionized water and anhydrous ethanol in a volume ratio of 1:

8. To the mixed solution, glacial acetic acid solution was added to adjust the pH to 5, ultrasonic dispersion was performed for 1 hour, γ-methacryloxypropyltrimethoxysilane was added, and the mixture was stirred and mixed to react, wherein the mass ratio of the mixed solution, the activated kaolin, and γ-methacryloxypropyltrimethoxysilane was 900:100:25, the reaction temperature was 85°C, and the reaction time was 6 hours. After the reaction, the mixture was cooled and centrifuged at a rate of 6000 r / min and a centrifugation time of 8 minutes. The mixture was washed with anhydrous ethanol and dried in a vacuum drying oven at 60°C for 24 hours to obtain olefinated kaolin.

3. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: In the step 2, the mass ratio of olefinated kaolin, ethyl acetate, itaconic acid and initiator is 100:1500-1800:72-90:1-3.

4. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: The reaction temperature in step 2 is 75-85° C. and the reaction time is 5-8 hours.

5. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: In the step 3, the mass ratio of carboxylated kaolin, N,N-dimethylformamide, 2,4,8,10-tetraoxa-3,9-diphosphospiro[5.5]undecane, 3,9-diamino, 3,9-dioxide, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride, 1-hydroxybenzotriazole, and triethylamine is 100:2500-3500:142-160:21-34:12-15:70-120, the reaction temperature is 30-35°C, and the reaction time is 8-10h.

6. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: In the step 4, the mass ratio of brominated butyl rubber, silicone rubber, flame retardant modified kaolin, antioxidant, lubricant, vulcanizing agent, magnesium oxide and zinc oxide is 100:25-40:4-9:0.5-1:1.2-2:1.5-3:0.5-1.2:0.8-1.

5.

7. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: In the step 4, the antioxidant includes one or more of antioxidant 168, antioxidant 1010, and p-aminodiphenylamine; the lubricant includes one or more of polyethylene wax, calcium stearate, and stearic acid; and the vulcanizing agent is composed of di-tert-butyl peroxyisopropylbenzene and vulcanization accelerator TMTD in a mass ratio of 1:

2.

8. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: In the step 4, the temperature of the first mixing is 75-85° C., the time of the first mixing is 30-35 min, the temperature of the second mixing is 100-120° C., and the time of the second mixing is 20-30 min.

9. The method for preparing a highly flame-retardant and highly heat-insulating composite material for a fire mask according to claim 1, characterized in that: The vulcanization temperature in step 4 is 170-180° C., and the vulcanization time is 10-18 minutes.

10. A highly flame retardant and highly thermally insulating composite material for fire masks prepared by the method for preparing a highly flame retardant and highly thermally insulating composite material for fire masks as described in any one of claims 1 to 9.