A kind of polyester-nylon composite rare earth antibacterial fiber and preparation method thereof
Through the synergy between carbon-based nanomaterials and rare earth ions, polyester composite rare earth antibacterial fibers were prepared, which solved the problem of moisture corrosion and static electricity of polyester composite fibers, achieved efficient and safe antibacterial effects, and improved the mechanical properties of the fibers and stability.
Patent Information
- Application Number
- CN202411179060.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing polyester composite fibers are prone to moisture, corrosion and serious electrostatic phenomena, resulting in bacterial growth. Traditional antibacterial agents have safety and stability problems.
Using the coordinated antibacterial of carbon-based nanomaterials and rare earth ions, rare earth antibacterial polyester slices and high viscosity copolyamide slices are prepared by in-situ polymerization to form polyester composite rare earth antibacterial fibers, using rare earth lanthanum, cerium, and yttrium ions The positive charge interferes with bacterial growth and destroys its structure.
It achieves efficient sterilization, safe, environmentally friendly, durable and insoluble antibacterial properties, and has good mechanical properties and dimensional stability, and is suitable for a variety of textiles.
Smart Images

Figure CN118704119B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a polyester-nylon composite rare earth antibacterial fiber and a preparation method thereof. Background Art
[0002] Polyester fiber, commonly known as polyester, is the largest variety of synthetic fiber at present. Polyester fiber is crisp and wrinkle-resistant, not easy to deform, has good shape retention, good dimensional stability, is easy to wash and dry quickly, but it also has the problems of low water absorption and poor moisture permeability.
[0003] Polyamide fiber, commonly known as nylon, is the first commercial synthetic fiber product of synthetic polymer. Polyamide fiber has the advantages of light weight, high strength, good wear resistance, resistance to weak acids and weak bases and some organic solvents, and easy molding and processing. However, it also has disadvantages such as high hygroscopicity, poor dimensional stability, easy wrinkling and deformation, low impact strength in dry state and low temperature, and poor resistance to strong acids and strong bases.
[0004] The preparation of polyester-nylon composite fiber is to prepare the composite fiber by the composite spinning method of two polymers, polyester and polyamide. It can combine the advantages of the two fibers, and has the advantages of good wear resistance, high strength, and easy dyeing of polyamide, and the advantages of polyester fiber such as crisp fabric, good shape retention, and no ironing. In addition, polyester fiber is cheap, and polyester-nylon composite fiber has certain advantages in cost compared with polyamide fiber. Polyester-nylon composite fiber is widely used in the industrial and textile fields, for example, it is used to make high-strength and high-toughness products, such as outdoor sports equipment, tents, backpacks, etc.; or it is used to make soft, tough and wrinkle-resistant textiles, such as bedding, shirts, etc.
[0005] Polyester-nylon composite fibers have many advantages, but they also have some disadvantages, such as being susceptible to moisture and corrosion, and being prone to static electricity. Due to static adsorption, the fiber surface absorbs a lot of dust, and combined with body fluids discharged from the human body and water vapor from the surrounding environment, bacteria are easily grown on the fiber surface. Therefore, the development of polyester-nylon composite fibers with antibacterial functions has great practical value.
[0006] The inorganic heavy metal antimicrobial agents commonly used in fibers, such as nano-silver, copper, and nano-zinc oxide, have significant antimicrobial properties, but they are dissolution-type antimicrobials, and the released heavy metal ions accumulate in the human body and the surrounding environment for a long time, which may cause certain harm. Natural antimicrobial agents are safe and environmentally friendly, but their antibacterial rate is average, their resistance to high temperature and discoloration is poor, and their stability is poor. Organic antimicrobial agents have good short-term rapid bactericidal effects, but most of them have poor thermal stability and poor washability, and their safety is still controversial.
[0007] China's rare earth resources are not only rich in reserves, but also have the advantages of complete mineral types and rare earth elements, and reasonable distribution of rare earth grades and mining sites. Through research, it is found that rare earth functional materials have an antibacterial rate of up to 100% against common Gram-positive and Gram-negative bacteria in life, and are safe, environmentally friendly, and have good biocompatibility. The application of rare earth materials in the field of antibacterial fibers has great application prospects. Summary of the invention
[0008] In view of this, the present invention aims to propose a polyester-nylon composite rare earth antibacterial fiber and a preparation method thereof. The present invention prepares a carbon-based nanomaterial doped with rare earth, and utilizes the high specific surface area and high porosity of the carbon-based nanomaterial to provide more doping active sites for the rare earth. The antibacterial performance of the material is improved by the synergistic antibacterial effect of the carbon-based nanomaterial and the rare earth ions. The polyester-nylon composite rare earth antibacterial fiber prepared by in-situ polymerization and composite melt spinning of the rare earth antibacterial polyester slice with a high-viscosity copolymer polyamide slice has good wear resistance, excellent mechanical properties, high strength and good dimensional stability, and is highly effective in sterilization and does not dissolve, is safe, environmentally friendly and durable, and can be used in outdoor sports equipment, tents, backpacks, socks, home textiles, bedding, shirts, home clothes and other fields.
[0009] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0010] A method for preparing polyester-nylon composite rare earth antibacterial fiber, the method comprising the following steps:
[0011] (1) Preparation of rare earth functional powders:
[0012] Take polyvinyl alcohol, deionized water, rare earth acetate compound, and polyvinyl pyrrolidone, put them into a reaction kettle and stir them evenly; add alkaline solution to adjust the pH to 8-12, reflux at 70-100°C, and continue stirring for 2-6 hours to obtain an intermediate product; put the intermediate product into an oven for drying, grind the dried intermediate product, and then add it into a muffle furnace for calcination to obtain a rare earth functional powder;
[0013] (2) Preparation of alcohol-based rare earth functional dispersion:
[0014] The rare earth functional powder and aliphatic diol are mixed evenly, and then a dispersant is added, and the mixture is evenly dispersed by multi-stage grinding in a sand mill to obtain an alcohol-based rare earth functional dispersion;
[0015] (3) Preparation of rare earth antibacterial polyester:
[0016] The alcohol-based rare earth functional dispersion, aliphatic diol, purified terephthalic acid, a stabilizer and a catalyst are prepared into a polymerization slurry, which is put into a high-pressure reactor for esterification and polycondensation reaction, and cooled and pelletized to obtain rare earth antibacterial polyester chips;
[0017] (4) Slice preprocessing:
[0018] The rare earth antibacterial polyester slices and the polyamide slices are dried separately, so that the moisture content of the rare earth antibacterial polyester slices is ≤50ppm, and the moisture content of the polyamide slices is ≤500ppm;
[0019] (5) Preparation of polyester-nylon composite rare earth antibacterial fiber:
[0020] The dried rare earth antibacterial polyester chips are added to the main screw extruder, and the dried polyamide chips are added to the auxiliary screw extruder. After high-temperature melting of the screw and metering by the metering pump, the melts of the two enter the main and auxiliary channels of the spinneret respectively for compounding, and then are extruded through the spinneret holes, cooled, oiled, stretched, and wound to obtain polyester-nylon composite rare earth antibacterial fibers.
[0021] Furthermore, the rare earth functional powder includes, by weight, 3-10 parts of polyvinyl alcohol, 80-200 parts of deionized water, 10-50 parts of rare earth acetate compound, and 1-10 parts of polyvinyl pyrrolidone.
[0022] Furthermore, the rare earth acetate compound is a mixture of lanthanum acetate, cerium acetate, and yttrium acetate, and the molar ratio thereof is 3-5: 2-4: 1-2;
[0023] The alkaline solution is one of sodium bicarbonate, sodium hydroxide, and ammonia.
[0024] Furthermore, in step (2), the mass ratio of rare earth functional powder, aliphatic diol and dispersant is (20-35):(62-79.5):(0.5-3), and the particle size of the alcohol-based rare earth functional dispersion is 100-500 nm.
[0025] Furthermore, the aliphatic diol in step (2) and step (3) is consistent, and the aliphatic diol is one of ethylene glycol, propylene glycol, and butanediol;
[0026] In step (3), the stabilizer is one of trimethyl phosphate, triphenyl phosphate, and triethyl phosphate; the catalyst is one of an antimony-based catalyst and a titanium-based catalyst; the molar ratio of purified terephthalic acid to aliphatic diol is 1:1.1-1.5; the mass of the stabilizer is 0.01-0.05% of the total mass of the polymerization slurry; the mass of the catalyst is 0.02-0.10% of the total mass of the polymerization slurry; and the equivalent rare earth functional powder accounts for 0.5%-3% of the total mass of the polymerization slurry.
[0027] Furthermore, in step (4), the polyamide slice is a high-viscosity copolyamide PA6-66, with a relative viscosity of 3.0-4.0 and a hot water extractable content of ≤0.5%.
[0028] High-viscosity copolyamide PA6-66 is prepared by adding the comonomer hexamethylenediamine adipate (commonly known as nylon 66 salt, abbreviated as HA-salt) into the PA6 polymerization, which can introduce [NH(CH2)6NHCO(CH2)4CO] chain segments into the PA6 chain structure and continuously prepare high-performance copolymer PA6-66. This material has better softness, higher transparency and more excellent mechanical properties while maintaining the unique excellent properties of PA6.
[0029] Furthermore, in step (5), the heating temperature of each zone of the main screw extruder is 270-300°C; the heating temperature of each zone of the secondary screw extruder is 260-300°C.
[0030] Furthermore, the fiber has a skin-core structure, the core layer is a high-viscosity copolymerized polyamide slice, and the skin layer is a rare earth antibacterial polyester slice.
[0031] Furthermore, the mass percentage of the skin layer is 30-70wt%.
[0032] The skin layer is selected as rare earth antibacterial polyester slice because it contains antibacterial functional components. Placing it in the skin layer can better play the antibacterial role. The antibacterial components can contact bacteria faster and more fully to achieve a rapid sterilization effect. High-viscosity copolyamide PA6-66 is selected as the core layer because of its excellent mechanical properties. Being in the core layer can provide better mechanical support for the composite matrix and improve the strength and wear resistance of the polymer material.
[0033] The present invention also provides a polyester-nylon composite rare earth antibacterial fiber prepared by any of the above-mentioned preparation methods.
[0034] Compared with the prior art, the polyester-nylon composite rare earth antibacterial fiber and the preparation method thereof described in the present invention have the following advantages:
[0035] 1. The rare earth functional powder prepared by the present invention is a carbon-based nanomaterial containing rare earth lanthanum / cerium / yttrium compounds. The high specific surface area and high porosity of carbon-based nanomaterials are used to provide more doping active sites for rare earths, and the antibacterial properties of the materials are improved through the synergistic antibacterial effect of carbon-based nanomaterials and rare earth ions. The antibacterial mechanism of rare earth lanthanum ions, cerium ions, and yttrium ions is similar. They carry positive charges. When they are electrostatically adsorbed on the surface of negatively charged bacterial cell membranes, they are antibacterial through the release and contact of metal ions, interfering with bacterial growth and hindering the transmission of nutrients. At the same time, they absorb energy from the environment, generate hydroxyl radicals and active oxygen ions, react with proteins, nucleic acids, glycosides, etc. in bacterial cells, destroy their normal structure, and eventually cause the bacteria to die or decompose.
[0036] 2. The antibacterial functional components are introduced into the polyester polymerization in the form of alcohol-based rare earth functional dispersion through in-situ polymerization. The antibacterial components have a strong binding force with the matrix, achieving a highly uniform dispersion of the rare earth antibacterial functional components in the polyester. The antibacterial properties of the antibacterial components can be fully exerted, ensuring the subsequent good spinnability and antibacterial durability.
[0037] 3. Antibacterial polyester slices containing antibacterial functional materials are used as the skin layer, and high-viscosity copolyamide slices are used as the core layer, which fully utilizes the strong antibacterial properties of the skin layer and the mechanical strength of the core layer, while also combining the good wear resistance, easy dyeing and good dimensional stability of polyester-nylon composite fibers.
[0038] 4. The prepared polyester-nylon composite rare earth fiber is highly effective in sterilization and does not dissolve. It is safe, environmentally friendly and durable. It can be used in outdoor sports equipment, tents, backpacks, socks, home textiles, bedding, shirts, home clothes and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0040] Figure 1 This is a flow chart for the preparation of polyester-nylon composite rare earth antibacterial fiber. DETAILED DESCRIPTION
[0041] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] A method for preparing polyester-nylon composite rare earth antibacterial fiber, the method comprising the following steps:
[0045] (1) Preparation of rare earth functional powders:
[0046] Weigh 4 parts of polyvinyl alcohol, 100 parts of deionized water, 25 parts of rare earth acetate compounds (the molar ratio of lanthanum acetate, cerium acetate and yttrium acetate is 3:3:1), and 2 parts of polyvinyl pyrrolidone by mass, put them into a reaction kettle and stir them evenly; add sodium bicarbonate to adjust the pH to 9, reflux at 90°C, and continue stirring for 4 hours to obtain an intermediate product; put the intermediate product into an oven and dry it at 110°C; grind the dried intermediate product and put it into a muffle furnace and calcine it at 1000°C for 2 hours to obtain a rare earth functional powder.
[0047] (2) Preparation of alcohol-based rare earth functional dispersion:
[0048] Weigh 25 parts of rare earth functional powder and 74 parts of ethylene glycol by mass and mix them evenly. Then add 1 part of dispersant polyvinyl pyrrolidone and grind them evenly in a sand mill to obtain a stable, non-settling alcohol-based rare earth functional dispersion with a particle size of 179 nm.
[0049] (3) Preparation of in-situ polymerized rare earth antibacterial polyester:
[0050] Alcohol-based rare earth functional dispersion, ethylene glycol, purified terephthalic acid, stabilizer trimethyl phosphate and catalyst ethylene glycol antimony are weighed by mass to prepare a polymerization slurry, which is put into a high-pressure reactor for esterification and polycondensation to obtain a rare earth antibacterial polyester melt, and the melt is cooled and pelletized to obtain rare earth antibacterial polyester chips PET with a characteristic viscosity of 1.15 dL / g.
[0051] The molar ratio of purified terephthalic acid to ethylene glycol in the slurry is 1:1.2, the mass of the stabilizer trimethyl phosphate is 0.03% of the total mass of the slurry, the mass of the catalyst ethylene glycol antimony is 0.04% of the total mass of the slurry, and the mass proportion of rare earth functional powder in the slurry is 2%.
[0052] The esterification reaction temperature is 250°C and the polycondensation reaction temperature is 280°C.
[0053] (4) Slice preprocessing:
[0054] The rare earth antibacterial polyester slices and high viscosity copolymer polyamide PA6-66 slices were dried separately, and the moisture content of the rare earth antibacterial polyester slices after drying was tested to be 30ppm, and the moisture content of the PA6-66 slices was 350ppm. The relative viscosity of the PA6-66 slices was 3.6.
[0055] (5) Preparation of polyester-nylon composite rare earth antibacterial fiber:
[0056] The composite rare earth antibacterial fiber has a skin-core structure, the skin layer is a rare earth antibacterial polyester slice, the core layer is a PA6-66 slice, and the mass ratio of the skin layer: the core layer component is 70:30.
[0057] The dried rare earth antibacterial polyester chips are added to the main screw extruder, and the dried PA6-66 chips are added to the auxiliary screw extruder. After high-temperature melting of the screw and metering by the metering pump, the melts of the two enter the main and auxiliary channels of the spinneret respectively for compounding, and then are extruded through the spinneret holes, cooled, oiled, stretched, and wound to obtain polyester-nylon composite rare earth antibacterial fibers.
[0058] The heating temperature of each zone of the main screw extruder is 290-300°C.
[0059] The heating temperature of each zone of the secondary screw extruder is 275-285°C.
[0060] Example 2
[0061] A method for preparing polyester-nylon composite rare earth antibacterial fiber, the method comprising the following steps:
[0062] (1) Preparation of rare earth functional powders:
[0063] Weigh 5 parts of polyvinyl alcohol, 130 parts of deionized water, 30 parts of rare earth acetate compounds (the molar ratio of lanthanum acetate, cerium acetate and yttrium acetate is 5:2:1), and 3 parts of polyvinyl pyrrolidone by mass, put them into a reaction kettle and stir them evenly; add sodium hydroxide to adjust the pH to 10, reflux at 90°C, and continue stirring for 5 hours to obtain an intermediate product; put the intermediate product into an oven and dry it at 130°C; grind the dried intermediate product and put it into a muffle furnace and calcine it at 1100°C for 3 hours to obtain a rare earth functional powder.
[0064] (2) Preparation of alcohol-based rare earth functional dispersion:
[0065] Weigh 30 parts of rare earth functional powder and 68 parts of propylene glycol by mass and mix them evenly. Then add 2 parts of dispersant polyvinyl pyrrolidone and grind them evenly in a sand mill to obtain a stable, non-settling alcohol-based rare earth functional dispersion with a particle size of 195 nm.
[0066] (3) Preparation of in-situ polymerized rare earth antibacterial polyester:
[0067] Alcohol-based rare earth functional dispersion, propylene glycol, purified terephthalic acid, stabilizer triphenyl phosphate and catalyst tetrabutyl titanate are weighed by mass to prepare a polymerization slurry, which is put into a high-pressure reactor for esterification and polycondensation to obtain a rare earth functional polyester melt. The melt is cooled and pelletized to obtain rare earth antibacterial polyester chips PTT with a characteristic viscosity of 0.72 dL / g.
[0068] The molar ratio of purified terephthalic acid and propylene glycol in the slurry is 1:1.3, the mass of the stabilizer triphenyl phosphate is 0.04% of the total mass of the slurry, the mass of the catalyst tetrabutyl titanate is 0.06% of the total mass of the slurry, and the mass of the rare earth functional powder in the slurry accounts for 3%.
[0069] The esterification reaction temperature is 255°C and the polycondensation reaction temperature is 285°C.
[0070] (4) Slice preprocessing:
[0071] The rare earth antibacterial polyester slices and PA6-66 slices were dried separately, and the moisture content of the rare earth antibacterial polyester slices after drying was tested to be 36ppm, and the moisture content of the PA6-66 slices was 400ppm. The relative viscosity of the PA6-66 slices was 3.0.
[0072] (5) Preparation of polyester-nylon composite rare earth antibacterial fiber:
[0073] The composite rare earth antibacterial fiber has a skin-core structure, the skin layer is a rare earth antibacterial polyester slice, the core layer is a PA6-66 slice, and the mass ratio of the skin layer: the core layer component is 60:40.
[0074] The dried rare earth antibacterial polyester chips are added to the main screw extruder, and the dried PA6-66 chips are added to the auxiliary screw extruder. After high-temperature melting of the screw and metering by the metering pump, the melts of the two enter the main and auxiliary channels of the spinneret respectively for compounding, and then extruded through the spinneret holes, cooled, oiled, stretched, and wound to obtain polyester-nylon composite rare earth antibacterial fibers. The heating temperature of each zone of the main screw extruder is 280-290°C.
[0075] The heating temperature of each zone of the secondary screw extruder is 265-275°C.
[0076] Example 3
[0077] A method for preparing polyester-nylon composite rare earth antibacterial fiber, the method comprising the following steps:
[0078] (1) Preparation of rare earth functional powders:
[0079] Weigh 6 parts of polyvinyl alcohol, 170 parts of deionized water, 40 parts of rare earth acetate compounds (the molar ratio of lanthanum acetate, cerium acetate and yttrium acetate is 3:2:2), and 5 parts of polyvinyl pyrrolidone by mass, put them into a reaction kettle and stir them evenly; add ammonia water to adjust the pH to 11, reflux at 100°C, and continue stirring for 5 hours to obtain an intermediate product; put the intermediate product into an oven and dry it at 140°C; grind the dried intermediate product and put it into a muffle furnace and calcine it at 1200°C for 4 hours to obtain a rare earth functional powder.
[0080] (2) Preparation of alcohol-based rare earth functional dispersion:
[0081] 33 parts of rare earth functional powder and 64 parts of butanediol were weighed by mass and mixed thoroughly, and then 3 parts of dispersant polyvinyl pyrrolidone were added, and multi-stage grinding and dispersion were performed in a sand mill to obtain a stable and non-settling alcohol-based rare earth functional dispersion with a particle size of 256 nm.
[0082] (3) Preparation of in-situ polymerized rare earth antibacterial polyester:
[0083] Alcohol-based rare earth functional dispersion, butanediol, purified terephthalic acid, stabilizer triethyl phosphate and catalyst tetraisopropyl titanate were weighed by mass to prepare a polymerization slurry, which was put into a high-pressure reactor for esterification and polycondensation to obtain a rare earth functional polyester melt. The melt was cooled and pelletized to obtain rare earth antibacterial polyester chips PBT with a characteristic viscosity of 0.90 dL / g.
[0084] The molar ratio of terephthalic acid to butanediol in the slurry is 1:1.4, the mass of the stabilizer triethyl phosphate is 0.05% of the total mass of the slurry, the mass of the catalyst tetraisopropyl titanate is 0.08% of the total mass of the slurry, and the mass of the rare earth functional powder in the slurry accounts for 2%.
[0085] The esterification reaction temperature is 245°C and the polycondensation reaction temperature is 290°C.
[0086] (4) Slice preprocessing:
[0087] The rare earth antibacterial polyester slices and PA6-66 slices were dried separately, and the moisture content of the rare earth antibacterial polyester slices after drying was tested to be 28ppm, and the moisture content of the PA6-66 slices was 320ppm. The relative viscosity of the PA6-66 slices was 3.2.
[0088] (5) Preparation of polyester-nylon composite rare earth antibacterial fiber:
[0089] The composite rare earth antibacterial fiber has a skin-core structure, the skin layer is a rare earth antibacterial polyester slice, the core layer is a PA6-66 slice, and the mass ratio of the skin layer: the core layer component is 50:50.
[0090] The dried rare earth antibacterial polyester chips are added to the main screw extruder, and the dried PA6-66 chips are added to the auxiliary screw extruder. After high-temperature melting of the screw and metering by the metering pump, the melts of the two enter the main and auxiliary channels of the spinneret respectively for compounding, and then are extruded through the spinneret holes, cooled, oiled, stretched, and wound to obtain polyester-nylon composite rare earth antibacterial fibers.
[0091] The heating temperature of each zone of the main screw extruder is 280-287°C.
[0092] The heating temperature of each zone of the secondary screw extruder is 270-280°C.
[0093] Comparative Example 1
[0094] The raw materials used for the skin layer and the core layer are replaced. The skin layer is PA6-66 slices, and the core layer is rare earth antibacterial polyester slices. The mass ratio of the skin layer: the core layer components is 30:70.
[0095] The heating temperature of each zone of the main screw extruder is 275-285° C. The heating temperature of each zone of the auxiliary screw extruder is 290-300° C. Others are the same as in Example 1.
[0096] Comparative Example 2
[0097] The mass ratio of the skin layer to the core layer is 90:10. Others are the same as in Example 1.
[0098] Comparative Example 3
[0099] The mass ratio of the skin layer to the core layer is 20:80. Others are the same as in Example 1.
[0100] Comparative Example 4
[0101] Weigh 5 parts of polyvinyl alcohol, 130 parts of deionized water, 30 parts of rare earth acetate compound (wherein the molar ratio of cerium acetate to yttrium acetate is 2:1), and 3 parts of polyvinyl pyrrolidone by mass, put them into a reaction kettle and stir them evenly; add sodium hydroxide to adjust the pH to 10, reflux at 90°C, and continue stirring for 5 hours to obtain an intermediate product; put the intermediate product into an oven and dry it at 130°C; grind the dried intermediate product and add it to a muffle furnace and calcine it at 1100°C for 3 hours to obtain a rare earth functional powder. Others are the same as in Example 2.
[0102] Comparative Example 5
[0103] Weigh 5 parts of polyvinyl alcohol, 130 parts of deionized water, 30 parts of rare earth acetate compound (wherein the molar ratio of lanthanum acetate to cerium acetate is 5:2), and 3 parts of polyvinyl pyrrolidone by mass, put them into a reaction kettle and stir them evenly; add sodium hydroxide to adjust the pH to 10, reflux at 90°C, and continue stirring for 5 hours to obtain an intermediate product; put the intermediate product into an oven and dry it at 130°C; grind the dried intermediate product and add it to a muffle furnace and calcine it at 1100°C for 3 hours to obtain a rare earth functional powder. Others are the same as in Example 2.
[0104] Comparative Example 6
[0105] Weigh 5 parts of polyvinyl alcohol, 130 parts of deionized water, 30 parts of rare earth acetate compound (wherein the molar ratio of lanthanum acetate to yttrium acetate is 5: 1), and 3 parts of polyvinyl pyrrolidone by mass, put them into a reaction kettle and stir them evenly; add sodium hydroxide to adjust the pH to 10, reflux at 90°C, and continue stirring for 5 hours to obtain an intermediate product; put the intermediate product into an oven and dry it at 130°C; grind the dried intermediate product and add it to a muffle furnace and calcine it at 1100°C for 3 hours to obtain a rare earth functional powder. Others are the same as in Example 2.
[0106] Comparative Example 7
[0107] Weigh 5 parts of polyvinyl alcohol, 130 parts of deionized water, 30 parts of rare earth acetate compounds (wherein the molar ratio of lanthanum acetate, cerium acetate, and yttrium acetate is 1:1:2), and 3 parts of polyvinyl pyrrolidone by mass, put them into a reaction kettle and stir them evenly; add sodium hydroxide to adjust the pH to 10, reflux at 90°C, and continue stirring for 5 hours to obtain an intermediate product; put the intermediate product into an oven and dry it at 130°C; grind the dried intermediate product and add it to a muffle furnace and calcine it at 1100°C for 3 hours to obtain a rare earth functional powder. Others are the same as in Example 2.
[0108] Comparative Example 8
[0109] 30 parts of rare earth sulfate compound (wherein the molar ratio of lanthanum sulfate, cerium sulfate and yttrium sulfate is 5:2:1) are used, and the rest is the same as in Example 2.
[0110] Comparative Example 9
[0111] 30 parts of rare earth nitrate compound (wherein the molar ratio of lanthanum nitrate, cerium nitrate and yttrium nitrate is 5:2:1) are used, and the rest is the same as in Example 2.
[0112] Test example:
[0113] The antibacterial properties and mechanical properties of the rare earth antibacterial fibers prepared in Examples 1-3 and Comparative Examples 1-9 were tested. The results are shown in Tables 1 and 2.
[0114] Table 1 Mechanical properties and antibacterial properties of the fibers of Examples 1-3
[0115]
[0116] Table 2 Mechanical properties and antibacterial properties of comparative fibers
[0117]
[0118] It can be seen from the data in the above table that the polyester-nylon composite rare earth antibacterial fiber prepared in Examples 1-3 has good antibacterial properties and excellent mechanical properties. The strong supporting effect of the high-viscosity copolyamide in the core layer improves the mechanical properties of the fiber. The concentration of the functional powder is adjusted by composite spinning technology, so that the fiber has good dimensional stability and excellent mechanical properties while taking into account the antibacterial properties. According to the washing method of 10.1.1 Washing color fastness tester in GB / T 20944.3-2008, after the fibers were washed 50 times, the fibers still had a high antibacterial rate, and the reduction was not very obvious, indicating that the polyester-nylon composite rare earth antibacterial fiber prepared by the present invention has washing resistance, high efficiency sterilization without dissolution, and strong antibacterial durability.
[0119] From the data of Example 1 and Comparative Example 1 in the above table, it can be seen that by changing the raw materials used for the skin layer and the core layer and using rare earth antibacterial polyester slices as the core layer, the antibacterial properties and mechanical properties are greatly reduced. Since it is wrapped in the inner layer, the antibacterial activity of the antibacterial component is not fully exerted, and the polyester as the core layer cannot provide a strong support effect, which reduces the mechanical strength of the fiber.
[0120] It can be seen from the data of Example 1 and Comparative Examples 2 and 3 in the above table that when the mass ratio of the cortex and the core layer components is changed beyond the specified range, the antibacterial properties or mechanical properties will be reduced, and the two cannot be taken into account. When the cortex accounts for 90 wt%, its mechanical strength is significantly reduced; when the cortex accounts for 20 wt%, its antibacterial properties are significantly reduced. This shows that within a certain mass ratio range, using antibacterial polyester slices as the cortex and high-viscosity copolyamide slices as the core layer can fully utilize the strong antibacterial properties of the cortex and the mechanical strength of the core layer, so that the fiber has both strong antibacterial properties and good mechanical properties.
[0121] From the data of Example 2 and Comparative Examples 4-7 in the above table, it can be seen that the antibacterial performance will deteriorate when the molar ratio or composition of the rare earth acetate compound is changed, which indicates that within an appropriate range, the carbon-based nanomaterials doped with rare earth lanthanum, cerium, and yttrium work together to improve the antibacterial performance of the material.
[0122] It can be seen from Example 2 and Comparative Examples 8-9 that the antibacterial activity becomes worse after replacing the rare earth acetate compounds with rare earth sulfate compounds and rare earth nitrate compounds. This is because acetate ions play a very important role in forming the carbon skeleton and fixing rare earth ions on the carbon skeleton. This is also the key to why rare earth acetate has stronger antibacterial and mechanical properties than rare earth nitrate and rare earth sulfate.
[0123] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing polyester-nylon composite rare earth antibacterial fiber, Features: The method comprises the following steps: (1) Preparation of rare earth functional powders: Take polyvinyl alcohol, deionized water, rare earth acetate compound, and polyvinyl pyrrolidone, put them into a reaction kettle and stir them evenly; add alkaline solution to adjust the pH to 8-12, reflux at 70-100°C, and continue stirring for 2-6 hours to obtain an intermediate product; put the intermediate product into an oven for drying, grind the dried intermediate product, and then add it into a muffle furnace for calcination to obtain a rare earth functional powder; (2) Preparation of alcohol-based rare earth functional dispersion: The rare earth functional powder and aliphatic diol are mixed evenly, and then a dispersant is added, and the mixture is evenly dispersed by multi-stage grinding in a sand mill to obtain an alcohol-based rare earth functional dispersion; (3) Preparation of rare earth antibacterial polyester: The alcohol-based rare earth functional dispersion, aliphatic diol, purified terephthalic acid, a stabilizer and a catalyst are prepared into a polymerization slurry, which is put into a high-pressure reactor for esterification and polycondensation reaction, and cooled and pelletized to obtain rare earth antibacterial polyester chips; (4) Slice preprocessing: The rare earth antibacterial polyester slices and the polyamide slices are dried separately, so that the moisture content of the rare earth antibacterial polyester slices is ≤50ppm, and the moisture content of the polyamide slices is ≤500ppm; (5) Preparation of polyester-nylon composite rare earth antibacterial fiber: The dried rare earth antibacterial polyester chips are added to the main screw extruder, and the dried polyamide chips are added to the auxiliary screw extruder. After high-temperature melting of the screw and metering by the metering pump, the melts of the two enter the main and auxiliary channels of the spinneret respectively for compounding, and then are extruded through the spinneret holes, cooled, oiled, stretched, and wound to obtain polyester-nylon composite rare earth antibacterial fibers. The rare earth acetate compound is a mixture of lanthanum acetate, cerium acetate and yttrium acetate, and the molar ratio thereof is 3-5: 2-4: 1-2; The fiber has a skin-core structure, the core layer is a high-viscosity copolymerized polyamide slice, and the skin layer is a rare earth antibacterial polyester slice; the mass percentage of the skin layer is 30-70wt%.
2. The method for preparing the polyester-nylon composite rare earth antibacterial fiber according to claim 1, Features: The rare earth functional powder comprises, by weight, 3-10 parts of polyvinyl alcohol, 80-200 parts of deionized water, 10-50 parts of rare earth acetate compound, and 1-10 parts of polyvinyl pyrrolidone.
3. The method for preparing the polyester-nylon composite rare earth antibacterial fiber according to claim 1, Features: The alkaline solution is one of sodium bicarbonate, sodium hydroxide, and ammonia.
4. The method for preparing the polyester-nylon composite rare earth antibacterial fiber according to claim 1, Features: In step (2), the mass ratio of rare earth functional powder, aliphatic diol and dispersant is (20-35): (62-79.5): (0.5-3), and the particle size of the alcohol-based rare earth functional dispersion is 100-500 nm.
5. The method for preparing the polyester-nylon composite rare earth antibacterial fiber according to claim 1, Features: The aliphatic diol in step (2) and step (3) is consistent, and the aliphatic diol is one of ethylene glycol, propylene glycol, and butanediol; In step (3), the stabilizer is one of trimethyl phosphate, triphenyl phosphate, and triethyl phosphate; the catalyst is one of an antimony-based catalyst and a titanium-based catalyst; the molar ratio of purified terephthalic acid to aliphatic diol is 1:1.1-1.5; the mass of the stabilizer is 0.01-0.05% of the total mass of the polymerization slurry; the mass of the catalyst is 0.02-0.10% of the total mass of the polymerization slurry; and the equivalent rare earth functional powder accounts for 0.5%-3% of the total mass of the polymerization slurry.
6. The method for preparing the polyester-nylon composite rare earth antibacterial fiber according to claim 1, Features: In step (4), the polyamide slice is a high-viscosity copolyamide PA6-66, the relative viscosity of which is 3.0-4.0, and the content of hot water extractable matter is ≤0.5%.
7. The method for preparing the polyester-nylon composite rare earth antibacterial fiber according to claim 1, Features: In step (5), the heating temperature of each zone of the main screw extruder is 270-300°C; the heating temperature of each zone of the secondary screw extruder is 260-300°C.
8. A polyester-nylon composite rare earth antibacterial fiber prepared by the preparation method according to any one of claims 1 to 7.