A repair process for damaged concrete floors based on pile foundation principles

By using a concrete floor repair process based on pile foundation principles, the surface slurry layer is cleaned and four curing treatments are carried out. Combined with the repair of deep pits and surface pits, the problems of uneven repair and easy damage in existing technologies are solved, and the overall solidity and wear resistance of the floor are achieved.

CN118704818BActive Publication Date: 2026-11-17SHANYI TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411185845.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2026-11-17
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing methods for repairing concrete floors vary, resulting in uneven color and poor bonding at the repaired areas. They are also prone to problems such as cracking, hollowing, and sanding, and cannot effectively extend the service life.

Method used

The repair process, based on the principle of pile foundation, includes cleaning the surface concrete slurry layer, four curing treatments, repair of deep and surface pits, and the use of semi-fast-setting semi-dry mortar and repair grout, combined with the use of alkaline curing agents to ensure uniformity and strength after each repair.

Benefits of technology

It achieves overall consistency and robustness of concrete flooring, avoids problems such as uneven color and poor structural bonding caused by local repairs, improves the hardness and wear resistance of the flooring, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118704818B_ABST
    Figure CN118704818B_ABST
Patent Text Reader

Abstract

This invention provides a repair process for damaged concrete floors based on the principle of pile foundations. It comprehensively repairs the damaged floor surface, utilizing the pile foundation principle to alter the surface structure of the repaired concrete floor, exposing the aggregate. This effectively disperses load-bearing pressure, transferring external pressure to the entire foundation layer, reducing surface stress and vibrations that could cause the entire floor to crack and peel. The repair process involves four curing treatments, with each layer reacting and curing from bottom to top. This results in better penetration and more complete reaction of the curing agent, thereby improving the floor's hardness and wear resistance, achieving a Mohs hardness of 7 or higher, and eliminating the risk of dusting. The use of a protective liquid reduces the floor's water absorption, providing anti-slip properties and slowing down the weathering rate of the concrete, further enhancing the floor's service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials and construction technology, and in particular to a repair process for damaged concrete floors based on the principle of pile foundation. Background Technology

[0002] Concrete floors are widely used in various buildings, including industrial, commercial, and residential buildings, due to their durability, dust and slip resistance, ease of cleaning, aesthetics, and wear resistance. However, in actual use, concrete floors can also experience problems such as cracking, hollowing, sanding, and peeling, which affect both the appearance and functionality of the floor and shorten its lifespan. In such cases, it is necessary to repair the concrete floor to address the specific issues.

[0003] Currently, the repair techniques for concrete floors typically involve addressing the affected area individually. For example, for localized cracks and pits, the options are either grout injection or partial resurfacing. Grout injection involves directly injecting repair material into the cracks or pits, providing quick results but leaving noticeable repair marks. Partial resurfacing, on the other hand, requires removing the repaired area down to the structural layer before re-pouring and hardening the concrete, leaving no visible repair marks but being more expensive and resulting in uneven coloring of the hardened concrete. Another example is addressing localized hollow areas in the concrete floor, which can be repaired by drilling holes, injecting grout into the hollow areas, and then re-grinding the surface.

[0004] The aforementioned repair methods vary depending on the specific concrete floor damage, resulting in overly targeted solutions. Even with partial repairs, the color of the repaired area often differs significantly from the rest of the floor. In practice, different problems frequently arise on the same concrete floor. Repairing using existing methods is time-consuming and produces unsightly results. Even after repair, firstly, the bond between the repaired area and the original floor is poor, making recurrence of problems easy; secondly, even repairs based on the existing concrete floor structure may still result in cracking, hollow areas, and sandblasting. Our company, considering the structural characteristics of concrete floors and based on the principles of pile foundations, has developed a new concrete floor repair process. Summary of the Invention

[0005] The purpose of this invention is to address the problems of unsightly and reduced performance after repair of damaged concrete floors, and the inability to solve the problems of cracking, hollowing, and sanding of concrete floors by restoring them according to the existing floor structure. Therefore, this invention proposes a repair process for damaged concrete floors based on the principle of pile foundation.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: A repair process for damaged concrete floors based on pile foundation principles includes the following steps: S1. Clean the surface concrete slurry layer; grind away the surface concrete slurry layer of the floor to be repaired until the aggregate in the concrete is exposed, and knock away any hollow parts. S2. First curing treatment: Remove dust from the cleaned floor surface, spray alkaline curing agent onto the floor at a rate of 0.6 kg per square meter, and keep it moist for more than 2 hours to allow it to undergo a natural hardening reaction for more than 18 hours. S3. Deep pit repair; pits exceeding 1 cm in diameter on the floor are considered deep pits. The deep pits are repaired using semi-fast-setting semi-dry mortar with 4-6 mm aggregate. The raw material ratio of the semi-fast-setting semi-dry mortar includes: 1 part 425# cement, 2 parts fine sand, 0.04 parts additives, 1.5 parts 4-6 mm aggregate, and 0.8 parts repair emulsion. S4. Surface pit repair; pits on the floor not exceeding 1 cm are surface pits. The surface pits are repaired with semi-fast-setting repair mortar containing concrete additives. The raw material ratio of the semi-fast-setting repair mortar includes: 1 part 425# cement, 2 parts fine sand, 0.04 parts additives, and 0.8 parts repair emulsion. S5. After the repair of deep and surface pits is completed, leave the pit for 24 hours. S6. Second curing treatment: Remove dust from the floor surface, spray alkaline curing agent onto the floor at a rate of 0.2 kg per square meter, and keep it moist for more than 2 hours, followed by continuous maintenance for 5 days. S7. Floor surface treatment; After maintenance is completed on the 6th day, grind off the repair mortar on the floor surface until the stones are evenly exposed; S8. Third curing treatment: Remove dust from the floor surface, spray alkaline curing agent onto the floor, using 0.15 kg per square meter of floor, and keep it moist for more than 2 hours; S9. Grind the floor to 300 mesh and remove surface dust; S10. Repair of small holes: Inspect the floor surface and repair any remaining small holes with repair slurry. The raw material ratio of the repair slurry includes: 1 part 425# cement, 0.03 parts additive, and 0.8 parts repair emulsion. S11, Fourth Curing Treatment: Three hours after repairing small holes, spray alkaline curing agent onto the floor, using 0.1 kg per square meter of floor surface. No moisturizing is required. S12. After the floor has been left to stand for 12 hours, grind it to 500 mesh, then grind it to 2000 mesh, clean it and let it dry. S13. Polishing treatment: Remove dust from the floor and apply a protective liquid evenly to the floor. After the protective liquid is applied, apply a polishing liquid evenly. After the polishing liquid has cured on the floor, keep the floor dry and use #4 and #5 pads to dry polish the floor surface in turn. S14, Inspect the floor surface and complete the floor repair.

[0007] Preferably, the repair operations in S3, S4, and S10 are all performed while the floor is moist; that is, For deep pit repair in step S3, the floor should be cleaned and moistened with a high-pressure gun before repair. Then, the semi-fast semi-dry mortar with 4-6 mm gravel should be sprayed on the entire surface while repairing. Repair should be carried out immediately after spraying. If the floor surface evaporates and returns to a dry state, the semi-fast semi-dry mortar should be sprayed again to ensure that the repaired area is always moist during the repair process. For surface pit repair in step S4, the semi-fast-setting semi-dry mortar in step S3 is replaced with the semi-fast-setting repair mortar containing concrete additives. Other operations are the same as in step S3 above. For the repair of small holes in step S10, the semi-fast-setting semi-dry mortar in step S3 is replaced with the repair grout, and the other operations are the same as in step S3 above.

[0008] Preferably, in step S4, for the repair of surface pits, the semi-fast-setting repair mortar with added concrete additives is mixed and then applied with a 4 mm notched trowel. Immediately after application, a defoaming roller is used to roll back and forth to defoam until a glossy concrete surface appears.

[0009] Preferably, in step S10, for the repair of small holes, the repair slurry is stirred and then applied to the ground with a putty knife to repair the remaining small holes. Depending on the situation, it is applied two to three times until no omissions are observed by the naked eye.

[0010] Preferably, if the tiny holes on the floor surface are too deep to be completely repaired by troweling, a grinding and grouting method is used in conjunction with a grinding machine for repair.

[0011] Preferably, each time the floor surface is dusted, the operation is to first suck up the dust from the floor, and then use a high-pressure water gun to wash the floor clean.

[0012] Preferably, in the four curing processes, the alkaline curing agent is a water-based inorganic sealing curing agent; the curing process includes the following steps: S101. Spray the alkaline curing agent evenly onto the floor surface and allow it to penetrate. S102. Observe the condition of the floor surface and promptly apply additional spray to any raised areas or areas with rapid penetration to ensure that the entire floor remains moistened by the alkaline hardener for at least 2 hours or other specified duration. S103. After most of the alkaline curing agent is absorbed by the concrete of the floor, it continuously pushes the remaining alkaline curing agent to evenly cover the floor surface until the amount of alkaline curing agent remaining on the floor surface remains basically unchanged. S104. Once the surface becomes slippery and thick underfoot, thoroughly rinse the entire floor surface with clean water, absorb the water, and wipe the floor dry to remove any residue of the alkaline hardener.

[0013] Preferably, in step S6, after the second curing treatment, the floor is continuously maintained for 5 days, and the floor is cleaned with a floor scrubber using weakly alkaline water every two days. Waxing or other sealing agents are not allowed on the floor surface.

[0014] Preferably, in steps S9 and S12, resin grinding discs of the corresponding mesh size are used to grind the floor, and water is sprayed evenly on the floor and cross-grinding is performed.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The repair process of this invention involves completely cleaning the concrete slurry layer (finishing layer) on the concrete floor surface until the aggregate is exposed. In step S7, the repair mortar on the floor surface is ground away until the stones are evenly exposed. Afterwards, grinding and polishing are performed directly, without re-covering the stones with a new concrete slurry layer. The exposed stones on the repaired concrete floor surface act like small piles standing in the concrete, effectively transmitting external pressure to the entire foundation layer of the floor, thereby reducing vibration caused by force applied to a specific point on the floor surface. Therefore, the newly repaired concrete floor structure of this invention can effectively avoid the risk of floor damage and peeling, extending its service life.

[0016] 2. The repair process of this invention removes all the original polishing layer on the concrete floor surface, exposing a relatively loose structural layer. This facilitates the penetration and soaking of the alkaline curing agent, hardens the cement mortar around the stones, and makes the bond between the stones and the cement sand tighter and stronger, thereby increasing the hardness and wear resistance of the floor.

[0017] 3. The repair process of this invention involves four curing treatments: before pothole repair, after pothole repair, after floor curing, before small hole repair, and after small hole repair. These four curing treatments ensure that the floor structure is well cured before and after each repair. The repeated alkaline curing treatment four times provides a multi-layer hardness enhancement effect compared to a single curing, resulting in an overall Mohs hardness of 7 or higher for the concrete floor. This enhances the floor's wear resistance, extends its service life, prevents dusting, and reduces the risk of cracking.

[0018] 4. The concrete slurry layer on the concrete floor surface is completely cleaned up to expose the aggregate. The entire floor is then re-cured and the surface is rebuilt. This can solve all damage problems, including cracking, hollowing, sanding, and peeling, in one go. The repaired floor has overall consistency and effectively avoids problems such as poor structural bonding and uneven color caused by using different repair methods for different problems. The repaired floor is aesthetically pleasing and more durable. Attached Figure Description

[0019] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the accompanying drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. The purpose of the drawings is to supplement the textual description with graphics, enabling people to intuitively and vividly understand each technical feature and the overall technical solution of the present invention, but they should not be construed as limiting the scope of protection of the present invention. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 This is a flowchart of a repair process for damaged concrete floors based on the principle of pile foundation. Detailed Implementation

[0021] To provide a further understanding of the purpose, structure, features, and functions of the present invention, this section will describe in detail specific embodiments of the present invention.

[0022] In the description of this invention, it should be noted that the terms "length", "width", "thickness", "center", "upper", "lower", "left", "right", "front", "rear", "vertical", "horizontal", "top", "bottom", "inner", and "outer" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0023] In the description of this invention, "several" means one or more, "many" means two or more, "greater than," "less than," "exceeding," etc. are understood to exclude the number itself, and "above," "below," "within," etc. are understood to include the number itself. Where "first" or "second" is used, it is only for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.

[0024] The following is for reference. Figure 1 The concrete floor repair process of the present invention will be described in detail below: A repair process for damaged concrete floors based on pile foundation principles includes the following steps: S1. Clean the surface concrete slurry layer; grind away the surface concrete slurry layer of the floor to be repaired until the aggregate in the concrete is exposed, and knock away any hollow parts. This step involves completely removing the concrete slurry layer from the floor surface, and simultaneously removing all problematic areas on the concrete slurry layer, including cracks, hollow areas, sand, and peeling, to perform a unified overall repair of the concrete floor.

[0025] S2. First curing treatment: Remove dust from the cleaned floor surface, spray alkaline curing agent onto the floor at a rate of 0.6 kg per square meter, and keep it moist for more than 2 hours to allow it to undergo a natural hardening reaction for more than 18 hours. The alkaline hardener sprayed in this step can directly reach the bottom of the loose layer of aggregate in the floor. After soaking, it can harden the loose cement mortar around the stones, allowing the stones to bond tightly with the cement and sand again, increasing the hardness of the concrete floor base layer, and providing a more solid foundation for subsequent repair work.

[0026] S3. Deep pit repair; pits exceeding 1 cm in diameter on the floor are considered deep pits. The deep pits are repaired using semi-fast-setting semi-dry mortar with 4-6 mm aggregate. The raw material ratio of the semi-fast-setting semi-dry mortar includes: 1 part 425# cement, 2 parts fine sand, 0.04 parts additives, 1.5 parts 4-6 mm aggregate, and 0.8 parts repair emulsion. In this step, 4-6 mm gravel is added to the repair mortar. The crushed gravel is used as aggregate to fill the deep pits, making the floor load-bearing capacity better and more uniform, effectively avoiding the problem of easy cracking at the deep pits caused by different stress on the floor.

[0027] In some embodiments, the 0.04 parts of additives in the semi-quick-setting semi-dry mortar can be selected from concrete additives, including one or more combinations of additive components such as plasticizers, water-reducing agents, tackifiers, and waterproofing agents, or commercially available pre-mixed concrete additive products. Plasticizers enhance the plasticity and deformability of concrete, facilitating construction and making the overall concrete structure more robust; water-reducing agents reduce the hydration reaction of concrete, thereby reducing the water content in the concrete, increasing its strength and hardness, making it easier to handle in construction, and reducing the amount of water required, thus lowering costs; tackifiers increase the viscosity of concrete, improve the uniformity of concrete mixing, enhance the durability of concrete, and reduce cracking; waterproofing agents prevent concrete leakage, while increasing the durability and weather resistance of concrete, and improving the stability and strength of concrete.

[0028] In some embodiments, 0.8 parts of the repair emulsion can be selected from concrete repair emulsions sold online. It is an aqueous dispersion of a high molecular polymer, which, when mixed with cement mortar, forms polymer cement mortar with excellent bonding, crack resistance, impermeability, wear resistance, and aging resistance.

[0029] S4. Surface pit repair; pits on the floor not exceeding 1 cm are surface pits. The surface pits are repaired with semi-fast-setting repair mortar containing concrete additives. The raw material ratio of the semi-fast-setting repair mortar includes: 1 part 425# cement, 2 parts fine sand, 0.04 parts additives, and 0.8 parts repair emulsion. In this step, relatively shallow surface pits on the floor are repaired. The repair mortar contains 0.04 parts concrete additive and 0.8 parts repair emulsion. Its composition can be the same as that of the concrete additive and repair emulsion in the above-mentioned S3 embodiment.

[0030] S5. After the repair of deep and surface pits is completed, allow it to stand for 24 hours to ensure that the repair material and the original flooring material fully react chemically to form a strong bond, thereby avoiding cracking and delamination and ensuring the strength and durability of the ground.

[0031] S6. Second curing treatment: Remove dust from the floor surface, spray alkaline curing agent onto the floor at a rate of 0.2 kg per square meter, and keep it moist for more than 2 hours, followed by continuous maintenance for 5 days. In this step, the amount of alkaline curing agent used is less than that used in the first curing treatment. This is because, firstly, the underlying structural layer has been cured in the first treatment, making it robust and eliminating the need for deeper penetration of the alkaline curing liquid into the floor. This layered curing method achieves better curing results and also reduces costs. After the second curing treatment, the concrete is cured for five consecutive days. This artificial curing allows the concrete to hydrate, gradually increasing its strength and ensuring the durability and stability of the floor.

[0032] S7. Floor surface treatment; After maintenance is completed on the 6th day, grind off the repair mortar on the floor surface until the stones are evenly exposed; This step is one of the key steps in the repair process of this invention. Grinding removes the stones until they are evenly exposed on the surface of the floor. These exposed stones act like small piles standing in the concrete, effectively transmitting external pressure to the entire foundation layer of the floor. This reduces vibrations caused by force applied to a single point on the floor surface. Therefore, the newly repaired concrete floor structure effectively avoids the risk of floor damage and peeling, extending its service life. It is this step that makes the surface structure of the repaired concrete floor completely different from the original. Traditional concrete floors have a concrete slurry layer that completely covers the stones, while the repaired concrete floor of this invention fully utilizes the pile foundation principle, resulting in a better stress transmission method, superior crack resistance, and a longer service life.

[0033] S8. Third curing treatment: Remove dust from the floor surface, spray alkaline curing agent onto the floor, using 0.15 kg per square meter of floor, and keep it moist for more than 2 hours; In this step, a third curing treatment is carried out between the operations of grinding and repairing the mortar and repairing small holes in the floor, which enhances the hardness and wear resistance of the floor and lays a good foundation for the repair of small holes.

[0034] S9. Roughly grind the floor to 300 mesh and remove surface dust; this facilitates the screening of small pores and further improves the smoothness of the floor surface.

[0035] S10. Repair of small holes: Inspect the floor surface and repair any remaining small holes with repair slurry. The raw material ratio of the repair slurry includes: 1 part 425# cement, 0.03 parts additive, and 0.8 parts repair emulsion. In this step, the repair slurry repairs smaller holes, thus further removing fine sand from the raw materials, resulting in a finer overall texture and better repair effect.

[0036] S11, Fourth Curing Treatment: 3 hours after the small hole repair, spray alkaline curing agent onto the floor, using 0.1 kg per square meter of floor, without moisturizing; this step is the last curing treatment using alkaline curing agent, and its purpose is to focus on curing the repaired small holes on the outermost layer.

[0037] S12. After the floor has been left to stand for 12 hours, grind it to 500 mesh, then grind it to 2000 mesh, clean it and let it dry. S13. Polishing treatment: Remove dust from the floor and apply a protective liquid evenly to the floor. After the protective liquid is applied, apply a polishing liquid evenly. After the polishing liquid has cured on the floor, keep the floor dry and use #4 and #5 pads to dry polish the floor surface in turn. S14, Inspect the floor surface and complete the floor repair.

[0038] This invention relates to a damaged concrete floor repair process that comprehensively repairs the damaged floor surface. Utilizing the principle of pile foundations, the repaired concrete floor surface structure is altered, exposing the aggregate and effectively dispersing load-bearing pressure. External pressure is transmitted to the entire base layer of the floor, reducing surface stress and vibrations that could cause damage and peeling. The repair process involves four curing treatments, with each layer reacting and curing from bottom to top. This results in better penetration and more complete reaction of the curing agent, thereby improving the floor's hardness and wear resistance, achieving a Mohs hardness of 7 or higher, and eliminating the risk of dusting. The use of a protective liquid reduces the floor's water absorption, providing anti-slip properties and slowing down the weathering rate of the concrete, further enhancing the floor's service life.

[0039] The four curing processes of this invention all use alkaline curing agents, which are suitable for most concrete floors. They can react chemically with alkaline substances in concrete to produce new compounds with more stable structures, forming a hard surface layer, thereby improving the hardness and wear resistance of the floor.

[0040] In some embodiments, the repair operations in S3, S4, and S10 are all performed while the floor is moist; that is... For deep pit repair in step S3, the floor should be cleaned and moistened with a high-pressure gun before repair. Then, the semi-fast semi-dry mortar with 4-6 mm gravel should be sprayed on the entire surface while repairing. Repair should be carried out immediately after spraying. If the floor surface evaporates and returns to a dry state, the semi-fast semi-dry mortar should be sprayed again to ensure that the repaired area is always moist during the repair process. For surface pit repair in step S4, the semi-fast-setting semi-dry mortar in step S3 is replaced with the semi-fast-setting repair mortar containing concrete additives. Other operations are the same as in step S3 above. For the repair of small holes in step S10, the semi-fast-setting semi-dry mortar in step S3 is replaced with the repair grout, and the other operations are the same as in step S3 above.

[0041] The repair process involves three stages, proceeding from bottom to top and from the inside out, following the order of deep pit repair, surface pit repair, and then small hole repair. As the size of the repaired holes decreases, the repair slurry becomes increasingly fine and smooth, facilitating subsequent grinding and polishing.

[0042] In some embodiments, in step S4, for repairing surface pits, the semi-fast-setting repair mortar with added concrete additives is mixed and then applied using a 4mm notched trowel. Immediately after application, a defoaming roller is used to roll back and forth to remove bubbles until a glossy concrete surface appears. In step S10, for repairing small holes, the repair slurry is mixed and then applied to the ground with a trowel to repair any remaining small holes. Depending on the situation, two to three applications are made, ensuring no areas are missed visually. This repair operation effectively reduces air bubbles in the concrete floor, ensuring uniform material application and a glossy surface, facilitating the reaction and curing of the alkaline hardener, and reducing surface sanding and cracking. Furthermore, if the small holes on the floor surface are too deep to be completely repaired by trowel application, a grinding and grouting method using a grinding machine is used for repair. The repair process of this invention involves repeated defoaming when repairing pits of various sizes, ensuring that the concrete slurry inside the floor is full and free of voids, while the surface is free of air bubbles, effectively guaranteeing the overall hardness and wear resistance of the floor.

[0043] In some embodiments, each time the floor surface is dusted, the operation is to first suck up the dust on the floor, and then use a high-pressure water gun to wash the floor clean. This cleaning is more thorough and also helps to moisturize and maintain the floor.

[0044] In some embodiments, a four-stage curing process is performed, wherein the alkaline curing agent is a water-based inorganic sealing curing agent; the curing process includes the following steps: S101. Spray the alkaline curing agent evenly onto the floor surface and allow it to penetrate. S102. Observe the condition of the floor surface and promptly apply additional spray to any raised areas or areas with rapid penetration to ensure that the entire floor remains moistened by the alkaline hardener for at least 2 hours or other specified duration. S103. After most of the alkaline curing agent is absorbed by the concrete of the floor, it continuously pushes the remaining alkaline curing agent to evenly cover the floor surface until the amount of alkaline curing agent remaining on the floor surface remains basically unchanged. S104. Once the surface becomes slippery and thick underfoot, thoroughly rinse the entire floor surface with clean water, absorb the water, and wipe the floor dry to remove any residue of the alkaline hardener.

[0045] In the curing process, the total amount of alkaline curing agent is calculated based on the concrete floor and the amount needed per square meter of floor. During actual spraying, the alkaline curing agent is evenly and fully penetrated into the floor according to the above operation, and sufficient curing reaction time is allowed. The resulting concrete floor not only has better hardness and wear resistance, but also a smoother and flatter surface.

[0046] In some embodiments, in step S6, after the second curing treatment, the floor is continuously maintained for 5 days, and the floor is cleaned with a floor scrubber using weakly alkaline water every two days. Waxing or other sealing agents are not allowed on the floor surface.

[0047] In some embodiments, in steps S9 and S12, resin grinding discs of the corresponding mesh size are used to grind the floor, and water is sprayed evenly on the floor and cross-grinding is performed.

[0048] In the above embodiments, the descriptions of each embodiment have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions of other embodiments.

[0049] The present invention has been described in the above-described embodiments. However, the above embodiments are merely examples for implementing the present invention and are used to help understand the technical solutions and core ideas of this application. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention; on the contrary, the technical solutions described in the foregoing embodiments can still be modified, or some of the technical features can be equivalently replaced; any modifications and refinements made without departing from the spirit and scope of the present invention are within the scope of patent protection of the present invention.

Claims

1. A process for repairing damaged concrete pavement based on the principle of pile foundation, characterized in that, Includes the following steps: S1. Clean the surface concrete slurry layer; grind away the surface concrete slurry layer of the floor to be repaired until the aggregate in the concrete is exposed, and knock away any hollow parts. S2. First curing treatment: Remove dust from the cleaned floor surface, spray alkaline curing agent onto the floor at a rate of 0.6 kg per square meter, and keep it moist for more than 2 hours to allow it to undergo a natural hardening reaction for more than 18 hours. S3. Deep pit repair: A pit exceeding 1 cm in diameter on the floor is considered a deep pit. The deep pit is repaired with semi-fast setting semi-dry mortar containing 4-6 mm of gravel. The raw material ratio of the semi-fast-setting semi-dry mortar includes: 1 part 425# cement, 2 parts fine sand, 0.04 parts additives, 1.5 parts 4-6 mm gravel, and 0.8 parts repair emulsion. S4. Surface pit repair; pits on the floor not exceeding 1 cm are surface pits. The surface pits are repaired with semi-fast-setting repair mortar containing concrete additives. The raw material ratio of the semi-fast-setting repair mortar includes: 1 part 425# cement, 2 parts fine sand, 0.04 parts additives, and 0.8 parts repair emulsion. S5. After the repair of deep and surface pits is completed, leave the pit for 24 hours. S6. Second curing treatment: Remove dust from the floor surface, spray alkaline curing agent onto the floor at a rate of 0.2 kg per square meter, and keep it moist for more than 2 hours, followed by continuous maintenance for 5 days. S7. Floor surface treatment; After maintenance is completed on the 6th day, grind off the repair mortar on the floor surface until the stones are evenly exposed; S8. Third curing treatment: Remove dust from the floor surface, spray alkaline curing agent onto the floor, using 0.15 kg per square meter of floor, and keep it moist for more than 2 hours; S9. Grind the floor to 300 mesh and remove surface dust; S10. Repair of small holes: Inspect the floor surface and repair any remaining small holes with repair slurry. The raw material ratio of the repair slurry includes: 1 part 425# cement, 0.03 parts additive, and 0.8 parts repair emulsion. S11, Fourth Curing Treatment: Three hours after repairing small holes, spray alkaline curing agent onto the floor, using 0.1 kg per square meter of floor surface. No moisturizing is required. S12. After the floor has been left to stand for 12 hours, grind it to 500 mesh, then grind it to 2000 mesh, clean it and let it dry. S13. Polishing treatment: Remove dust from the floor and apply a protective liquid evenly to the floor. After the protective liquid is applied, apply a polishing liquid evenly. After the polishing liquid has cured on the floor, keep the floor dry and use #4 and #5 pads to dry polish the floor surface in turn. S14, Inspect the floor surface and complete the floor repair; In the four curing processes, the alkaline curing agent is a water-based inorganic sealing and curing agent; the curing process includes the following steps: S101. Spray the alkaline curing agent evenly onto the floor surface and allow it to penetrate. S102. Observe the condition of the floor surface and promptly apply additional spray to any raised areas or areas with rapid penetration to ensure that the entire floor remains moistened by the alkaline hardener for at least 2 hours or other specified duration. S103. After most of the alkaline curing agent is absorbed by the concrete of the floor, it continuously pushes the remaining alkaline curing agent to evenly cover the floor surface until the amount of alkaline curing agent remaining on the floor surface remains basically unchanged. S104. Once the surface becomes slippery and thick underfoot, thoroughly rinse the entire floor surface with clean water, absorb the water, and wipe the floor dry to remove any residue of the alkaline hardener.

2. The process for repairing damaged concrete pavement based on the principle of pile foundation as claimed in claim 1, wherein: The repair operations in S3, S4, and S10 are all carried out while the floor is moist; that is... For deep pit repair in step S3, the floor should be cleaned and moistened with a high-pressure gun before repair. Then, the semi-fast semi-dry mortar with 4-6 mm gravel should be sprayed on the entire surface while repairing. Repair should be carried out immediately after spraying. If the floor surface evaporates and returns to a dry state, the semi-fast semi-dry mortar should be sprayed again to ensure that the repaired area is always moist during the repair process. For surface pit repair in step S4, the semi-fast-setting semi-dry mortar in step S3 is replaced with the semi-fast-setting repair mortar containing concrete additives. Other operations are the same as in step S3 above. For the repair of small holes in step S10, the semi-fast-setting semi-dry mortar in step S3 is replaced with the repair grout, and the other operations are the same as in step S3 above.

3. The process for repairing damaged concrete pavement based on the principle of pile foundation as claimed in claim 2, wherein: In step S4, for the repair of surface pits, the semi-fast-setting repair mortar with concrete additives is mixed and then applied with a 4 mm notched trowel. Immediately after application, a defoaming roller is used to roll back and forth to defoam until a glossy concrete surface appears.

4. The process for repairing damaged concrete pavement based on the principle of pile foundation as claimed in claim 2, wherein: In step S10, for the repair of small holes, the repair slurry is stirred and then applied to the ground with a putty knife to repair the remaining small holes. Depending on the situation, it is applied two to three times until no omissions are observed by the naked eye.

5. The process for repairing damaged concrete pavement based on the principle of pile foundation as claimed in claim 4, wherein: If the tiny holes on the floor surface are too deep to be completely repaired by trowel, then a grinding and grouting method can be used in conjunction with a grinding machine for repair.

6. The process for repairing damaged concrete pavement based on the principle of pile foundation as claimed in claim 1, wherein: Each time the floor surface is dusted, the procedure is to first suck up the dust from the floor, and then use a high-pressure water gun to wash the floor clean.

7. The repair process for damaged concrete floors based on the pile foundation principle as described in claim 1, characterized in that: In step S6, after the second curing treatment, the floor is continuously maintained for 5 days. Every two days, the floor is cleaned with a floor scrubber using weak alkaline water. Waxing or other sealing agents are not allowed on the floor surface.

8. The repair process for damaged concrete floors based on the pile foundation principle as described in claim 1, characterized in that: In steps S9 and S12, the floor is polished using resin grinding discs of the appropriate mesh size, and water is sprayed evenly on the floor and then cross-polished.

Citation Information

Patent Citations

  • Concrete millstone terrace

    CN110656753A

  • Whole-course dust-free dry-grinding environment-friendly construction method for solidified terrace

    CN114687531A