A low-cost manganese-rich iron-based sodium ion battery positive electrode material and its preparation method and application

By doping large-particle metal elements into the positive electrode material of ferromanganese-rich sodium ion battery, expanding the sodium layer spacing, the problem of poor rate performance caused by iron clusters is solved, and a high rate performance and low-cost positive electrode material of sodium ion battery is achieved , suitable for large-scale production.

CN118712387BActive Publication Date: 2024-11-19TIANJIN GUOAN MGL NEW MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411179076.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-19
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The existing positive electrode materials of ferromanganese-rich sodium manganese-based battery have high iron content, resulting in iron cluster formation, reduced migration energy barrier, resulting in poor sodium ion mixing and rate performance, limiting its application.

Method used

By doping large-particle metal elements A, B, C (such as Y, La, Sr, Cd, K, Ca, Ba), expanding the sodium layer spacing, improving the diffusion rate and rate performance of sodium ions, a simple sintering preparation method is adopted , suitable for large-scale production.

Benefits of technology

It effectively improves the rate performance of the positive electrode material of sodium ion battery and reduces production costs, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118712387B_ABST
    Figure CN118712387B_ABST
Patent Text Reader

Abstract

The present invention relates to a low-cost manganese-rich iron-based sodium ion battery positive electrode material and a preparation method and application thereof. The chemical general formula of the positive electrode material is Na u Fe 1‑x Mn x M y O 2 , of which 0.98
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a low-cost manganese-rich iron-based sodium ion battery positive electrode material and a preparation method and application thereof. Background Art

[0002] Sodium is the second lightest element in the world. From the perspective of the periodic table, sodium and lithium belong to the same group of elements, and their physical and chemical properties are very similar. Although lithium-ion batteries have an advantage over sodium-ion batteries in terms of energy density, sodium storage resources are much higher than lithium, and its market price is much lower than lithium. Therefore, for large-scale applications in the energy storage and electric vehicle industries, sodium-ion batteries have the advantages of low cost and abundant resources, and are considered to be a new energy storage battery system that is very likely to replace lithium batteries.

[0003] Layered transition metal oxides are the most promising cathode materials for sodium ion batteries. They have become a hot topic in current research because of their high theoretical specific capacity, good low temperature performance and fast diffusion kinetics. Sodium-electric iron-manganese binary cathode materials have more cost advantages than traditional nickel-containing materials, but in order to ensure a higher capacity, the iron content in the material is also higher. The increased iron content will form iron clusters, and the migration energy barrier will be reduced, resulting in the iron-manganese binary material charging and discharging process. The iron will migrate into the sodium layer and mix with the sodium atoms, and the material rate performance will become very poor. Due to its poor rate performance, its use is severely restricted. Therefore, the present invention considers expanding its interlayer spacing by doping with large-particle elements to obtain a new low-cost and high-rate performance manganese-rich iron-based binary material. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a manganese-rich iron-based sodium ion battery positive electrode material and a preparation method and application thereof. The present invention expands the interlayer spacing of the manganese-rich iron-based sodium ion battery positive electrode material by selecting large-particle metal additives A element, B element and C element, which helps to increase the diffusion rate of sodium ions and further improve the rate performance of the positive electrode material; and the preparation method provided by the present invention is simple and easy to operate, has low requirements on the production process, and is conducive to large-scale production.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In the first aspect, the present invention provides a low-cost manganese-rich iron-based sodium ion battery positive electrode material, the positive electrode material has a chemical formula of Na u Fe 1-x Mn x M yO2, where 0.98 < u ≤ 1.05, 0.5 ≤ x ≤ 0.75, 0.03 ≤ y ≤ 0.2, the doping element M includes element A, element B and element C, where element A includes Y and / or La, element B includes Sr, and element C includes any one or a combination of at least two of Cd, K, Ca or Ba, and the sodium layer spacing d of the positive electrode material satisfies 5.45 Å ≤ d ≤ 5.55 Å.

[0007] Among them, u can be 0.99, 1, 1.01, 1.02, 1.03, 1.04 or 1.05, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable; x can be 0.5, 0.55, 0.6, 0.65, 0.7 or 0.75, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable; y can be 0.03, 0.05, 0.1, 0.15, 0.19 or 0.2, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable; d can be 5.45 Å, 5.47 Å, 5.49 Å, 5.51 Å, 5.53 Å or 5.55 Å, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.

[0008] Typical but non-limiting combinations of element C include the combination of Cd and K, or the combination of K, Ca and Ba; typical but non-limiting combinations of the doping element M include the combination of Y, Sr and Cd, or the combination of La, Sr and K, or the combination of La, Sr, Ca and Ba.

[0009] The present invention uses a manganese-rich iron-based sodium-ion battery positive electrode material as a matrix, and selects large-particle-size metal additive element A, element B and element C with an ionic radius of 90×10 -12 -140×10 -12 m for doping, where element A includes Y and / or La, element B includes Sr, and element C includes any one or a combination of at least two of Cd, K, Ca or Ba. Among them, La / Y enters the transition metal layer to form strong La / Y-O bonds, which increases the repulsion force between oxygen atoms in the sodium layer, and then increases the layer spacing of the sodium layer; Sr will enter the Na layer, playing a "supporting" role while also having a fluxing effect to help large-particle-size atoms doped into the material structure; Cd, K, Ca or Ba will enter the Na layer, playing a "supporting" role, and due to its large radius, it expands the layer spacing of the sodium layer. The synergistic effect of large-particle-size metal ions entering the material expands the layer spacing of the positive electrode material, improves the sodium-ion diffusion rate, and further improves the rate performance of the positive electrode material.

[0010] The present invention selects to dope element A, element B and element C, and through the synergistic effect of these three elements, effectively expands the layer spacing of the sodium layer.

[0011] After the positive electrode material prepared by the present invention is tested by XRD, the interlayer spacing d can be calculated by the Bragg equation 2dsinθ=nλ (d: crystal plane distance; θ: diffraction angle; λ: X-ray wavelength; n is the reflection order). The interlayer spacing of the positive electrode material not doped with elements A, B and C is 5.34Å, which further shows that the interlayer spacing of the manganese-rich iron-based sodium ion battery positive electrode material is increased after being co-doped with elements A, B and C.

[0012] The doping element M in the present invention is preferably a combination of Y, Sr and Cd, and the molar ratio of the three doping elements is further preferably (1-2):1:1, for example, it can be 1:1:1, 1.5:1:1, 1.9:1:1 or 2:1:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] In a second aspect, the present invention provides a method for preparing the positive electrode material as described in the first aspect, the preparation method comprising the following steps:

[0014] Mixing an iron-manganese source, a sodium source and a dopant, and sintering to obtain the positive electrode material;

[0015] The dopant includes a doping element M, M includes an A element, a B element and a C element, wherein the A element includes Y and / or La, the B element includes Sr, and the C element includes any one of Cd, K, Ca or Ba or a combination of at least two thereof.

[0016] The present invention can prepare a low-cost manganese-rich iron-based sodium ion battery positive electrode material through one-step sintering. The preparation method is simple and easy to operate, has low requirements on the production process, and is conducive to large-scale production.

[0017] Preferably, said mixing comprises stirring.

[0018] Preferably, the mixing rotation speed is 300-1300 r / min, for example, it can be 300 r / min, 500 r / min, 700 r / min, 900 r / min or 1300 r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the mixing time is 10-30 min, for example, 10 min, 15 min, 20 min, 25 min or 30 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the iron-manganese source comprises any one or a combination of at least two of an iron-manganese hydroxide precursor, an iron-manganese oxide or an iron-manganese carbonate. Typical but non-limiting combinations include a combination of an iron-manganese oxide and an iron-manganese hydroxide precursor, and a combination of an iron-manganese oxide, an iron-manganese hydroxide precursor and an iron-manganese carbonate.

[0021] Preferably, the iron manganese hydroxide precursor is prepared by the following preparation method:

[0022] Iron salt and manganese salt are weighed in an iron-manganese molar ratio, respectively, and dissolved in deionized water, to which carbon nanotubes, sodium hydroxide solution and ammonia water are added in sequence to obtain a mixed solution; the mixed solution is dried in an oven to obtain the iron-manganese hydroxide precursor.

[0023] Preferably, the chemical formula of the iron manganese hydroxide precursor is Fe 1-x Mn x (OH)2, wherein 0.5≤x≤0.75, for example, it can be 0.5, 0.55, 0.6, 0.65, 0.7 or 0.75, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] Preferably, the iron salt comprises any one of ferrous sulfate heptahydrate, ferrous sulfate monohydrate or anhydrous ferrous sulfate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of ferrous sulfate heptahydrate and ferrous sulfate monohydrate, or a combination of ferrous sulfate heptahydrate, ferrous sulfate monohydrate and anhydrous ferrous sulfate.

[0025] Preferably, the manganese salt comprises manganese sulfate monohydrate and / or anhydrous manganese sulfate.

[0026] Preferably, the drying temperature is 100-140° C., for example, 100° C., 120° C., 130° C. or 140° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] Preferably, the drying time is 8-12 hours, for example, 8 hours, 9 hours, 10 hours, 11 hours or 12 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the sodium source comprises sodium carbonate and / or sodium bicarbonate.

[0029] Preferably, the mass ratio of the A element, the B element and the C element is (0.5-2):(1-2):1, for example, it can be 0.5:1:1, 1:1:1, 1.5:2:1 or 2:1:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the A element includes Y, the B element includes Sr, and the C element includes Cd.

[0031] Preferably, the dopant includes an A dopant, a B dopant and a C dopant.

[0032] Preferably, the A dopant includes an yttrium source and / or a lanthanum source, the B dopant includes a strontium source, and the C dopant includes any one or a combination of at least two of a cadmium source, a potassium source, a calcium source or a barium source. Typical but non-limiting combinations include a combination of a cadmium source and a potassium source, or a combination of a potassium source, a calcium source and a barium source.

[0033] Preferably, the A dopant includes a yttrium source, the B dopant includes a strontium source, and the C dopant includes a cadmium source.

[0034] Preferably, the yttrium source comprises yttrium oxide and / or yttrium carbonate.

[0035] Preferably, the lanthanum source comprises lanthanum oxide and / or lanthanum carbonate.

[0036] Preferably, the strontium source comprises strontium oxide and / or strontium carbonate.

[0037] Preferably, the cadmium source comprises cadmium oxide and / or cadmium carbonate.

[0038] Preferably, the potassium source comprises potassium carbonate.

[0039] Preferably, the calcium source comprises calcium oxide and / or calcium carbonate.

[0040] Preferably, the barium source comprises barium oxide and / or barium carbonate.

[0041] Preferably, typical but non-limiting combinations of the dopants include a combination of a yttrium source, a strontium source and a cadmium source, or a combination of a lanthanum source, a strontium source and a potassium source, or a combination of a lanthanum source, a strontium source, a calcium source and a barium source.

[0042] Preferably, the dopant comprises a yttrium source, a strontium source and a cadmium source.

[0043] Preferably, the sintering temperature is 940-1200°C, for example, 940°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the sintering time is 10-14 h, for example, 10 h, 10.5 h, 11 h, 11.5 h, 12 h, 13 h or 14 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Within the temperature and sintering time range, a positive electrode material with uniform particle size distribution is prepared. When the sintering time becomes longer or the temperature increases, the material particles will grow. On the one hand, the specific surface area will decrease as the particles grow, thereby reducing side reactions and enhancing stability. At the same time, the sodium reaction sites will decrease due to the reduction in specific surface area, and the capacity will decrease. When the temperature exceeds 1200°C, the specific surface area is too small, and the extraction and embedding of sodium ions are seriously affected, thereby affecting the rate performance of the positive electrode material. When the sintering time becomes shorter or the temperature decreases, the capacity will decrease due to insufficient reaction, the crystal surface becomes rough, the grains are not round, and the grain tips are easily deactivated during the reaction process, which also affects the long-term cycle performance of the material.

[0046] Preferably, the sintering atmosphere includes an oxygen-containing atmosphere.

[0047] Preferably, the oxygen-containing atmosphere comprises air, oxygen or any atmosphere containing oxygen.

[0048] Preferably, the sintering heating rate is 4-5 min / °C, for example, it can be 4 min / °C, 4.2 min / °C, 4.4 min / °C, 4.6 min / °C, 4.8 min / °C or 5 min / °C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0049] The sintering cooling rate is 3-5 min / °C, for example, 3 min / °C, 3.5 min / °C, 4 min / °C, 4.5 min / °C or 5 min / °C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] Preferably, the sintering is followed by a crushing and screening process.

[0051] Preferably, after the crushing and screening, the particle size D50 of the positive electrode material is 4-8 μm, for example, 4 μm, 5 μm, 6 μm, 7 μm or 8 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] In a third aspect, the present invention provides a sodium ion battery, comprising the positive electrode material described in the first aspect, or the positive electrode material prepared by the preparation method described in the second aspect.

[0053] Compared with the prior art, the present invention has at least the following beneficial effects:

[0054] (1) The present invention dopes large-particle metal ions into the manganese-rich iron-based sodium ion battery positive electrode material. These ions do not participate in the electrochemical reaction, but help to expand the interlayer spacing of the iron-manganese material, and further help to increase the sodium ion diffusion rate, so as to obtain a manganese-rich iron-based sodium ion battery positive electrode material with high rate performance;

[0055] (2) The present invention can prepare a low-cost manganese-rich iron-based sodium ion battery positive electrode material through a one-step sintering process. The preparation method is simple and easy to operate, has low requirements on the production process, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 is a SEM image of the positive electrode material prepared in Example 1;

[0057] Figure 2 This is the charge and discharge curve of the positive electrode material prepared in Example 1. DETAILED DESCRIPTION

[0058] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0059] Example 1

[0060] This embodiment provides a low-cost manganese-rich iron-based sodium ion battery positive electrode material, and the preparation method of the positive electrode material is as follows:

[0061] Weigh 139g of ferrous sulfate heptahydrate and 84.5g of manganese sulfate monohydrate, add 300ml of deionized water, then add 10g of 14% carbon nanotube solution, mix well, add 20% ammonia water to pH=6, add 0.1mol / L sodium hydroxide to pH=11, and dry at 120℃ for 8h to prepare iron manganese hydroxide precursor Fe0.5Mn0.5(OH)2;

[0062] Weigh 89.39 g of Fe0.5Mn0.5(OH)2, a precursor of iron manganese hydroxide, 53 g of sodium carbonate, 6.78 g of yttrium oxide, 8.88 g of strontium carbonate and 7.68 g of cadmium oxide, stir at 300 r / min for 15 min to obtain a mixed material; sinter the mixed material at 1000°C for 12 h under an oxygen atmosphere, crush and sieve to obtain Na1Fe0.5Mn0.5Y0.06Sr0.06Cd0.06O2;

[0063] Figure 1 This is a SEM image of the positive electrode material prepared in Example 1. It can be seen from the image that the sintered particles are independent and not secondary particles, and the particle size of the grains is mostly between 4-8 μm;

[0064] Figure 2This is the charge and discharge curve of the positive electrode material prepared in Example 1. It can be seen from the figure that the first charge capacity of the 2-4V material at 0.1C is about 150mAh / g, and the first discharge reaches more than 140mAh / g, with excellent electrochemical performance.

[0065] Example 2

[0066] This embodiment provides a low-cost manganese-rich iron-based sodium ion battery positive electrode material, and the preparation method of the positive electrode material is as follows:

[0067] Weigh 20g of iron oxide, 65.21g of manganese dioxide, 88.2g of sodium bicarbonate, 11.3g of yttrium oxide, 7.4g of strontium carbonate and 3.45g of potassium carbonate, and stir at 800r / min for 25min to obtain a mixed material; sinter the mixed material at 1200°C for 10h in an air atmosphere, and crush and sieve to prepare Na1.05Fe0.25Mn0.75Y0.1Sr0.05K0.05O2.

[0068] Example 3

[0069] This embodiment provides a low-cost manganese-rich iron-based sodium ion battery positive electrode material, and the preparation method of the positive electrode material is as follows:

[0070] Weigh 46.32 g of ferrous carbonate, 69 g of manganese carbonate, 52.47 g of sodium carbonate, 8.15 g of lanthanum oxide, 7.4 g of strontium carbonate and 7.67 g of barium oxide, and stir at 500 r / min for 20 min to obtain a mixed material; sinter the mixed material at 940°C for 14 h under an air atmosphere, and crush and sieve to prepare Na0.99Fe0.4Mn0.6La0.05Sr0.05Ba0.05O2.

[0071] Example 4

[0072] The only difference between this embodiment and embodiment 1 is that, except for adding 1.48 g of strontium carbonate, 1.28 g of cadmium oxide and 1.13 g of yttrium oxide to prepare Na1Fe0.5Mn0.5Y0.01Sr0.01Cd0.01O2, the rest is the same as embodiment 1.

[0073] Example 5

[0074] The only difference between this embodiment and embodiment 1 is that, except for adding 1.48 g of strontium carbonate to prepare Na1Fe0.5Mn0.5Y0.06Sr0.01Cd0.06O2, the rest is the same as embodiment 1.

[0075] Example 6

[0076] The only difference between this embodiment and embodiment 1 is that, except for the sintering temperature of 900° C., the rest is the same as embodiment 1.

[0077] Example 7

[0078] The difference between this embodiment and embodiment 1 is that, except for the sintering temperature of 1250° C., the rest is the same as embodiment 1.

[0079] Example 8

[0080] The only difference between this embodiment and embodiment 1 is that, except for the sintering time of 9.5 hours, the rest is the same as embodiment 1.

[0081] Example 9

[0082] The difference between this embodiment and embodiment 1 is that, except for the sintering time of 14.5 hours, the rest is the same as embodiment 1.

[0083] Comparative Example 1

[0084] The difference between this comparative example and Example 1 is that, except that yttrium oxide, strontium carbonate and cadmium oxide are not added, the rest is the same as Example 1.

[0085] Comparative Example 2

[0086] The difference between this comparative example and Example 1 is that, in addition to adding 4.86g zinc oxide, 4.74g copper oxide and 4.5g cobalt oxide to prepare Na1Fe0.5Mn0.5Zn0.06Cu0.06Co0.06O2, the rest is the same as Example 1.

[0087] Comparative Example 3

[0088] The difference between this comparative example and Example 1 is that, except for adding only 6.78 g of yttrium oxide to prepare Na1Fe0.5Mn0.5Y0.06O2, the rest is the same as Example 1.

[0089] Comparative Example 4

[0090] The difference between this comparative example and Example 1 is that, except for adding only 8.88 g of strontium carbonate to prepare Na1Fe0.5Mn0.5Sr0.06O2, the rest is the same as Example 1.

[0091] Comparative Example 5

[0092] The difference between this comparative example and Example 1 is that, except for adding only 7.68 g of cadmium oxide to prepare Na1Fe0.5Mn0.5Cd0.06O2, the rest is the same as Example 1.

[0093] Comparative Example 6

[0094] The difference between this comparative example and Example 1 is that, except that cadmium oxide is not added and Na1Fe0.5Mn0.5Y0.06Sr0.06O2 is prepared, the rest is the same as Example 1.

[0095] Test Method

[0096] The positive electrode materials prepared in Examples 1-9 and Comparative Examples 1-6 were subjected to XRD test and rate test. The test method of the rate test was as follows: the prepared iron-manganese binary material was mixed with conductive carbon black and binder polyvinylidene fluoride (PVDF) in a mass ratio of 85:10:5, N-methylpyrrolidone (NMP) was added and stirred evenly, coated on aluminum foil, placed in an oven for 8 hours and dried at 100°C, the material electrode sheet was cut as the positive electrode, the metal sodium sheet was the negative electrode, the electrolyte was a mixed system containing 1M NaPF6 (DEC:EC:FEC) / (volume ratio of 2:3:5), the diaphragm was glass fiber (Waterman), and assembled into a 2032 button cell in an argon (Ar) protected glove box. The battery was tested in the voltage range of 2.0-4.0V, and the charge and discharge cycles were 5 weeks at 0.1C / 0.5C / 1C / 2C respectively;

[0097] According to the XRD test results, the sodium interlayer spacing d of the positive electrode material is calculated and recorded in Table 1, and the test results of the rate performance are also recorded in Table 1.

[0098] Table 1

[0099]

[0100] The test results show that:

[0101] (1) It can be seen from Examples 1-9 and Comparative Examples 1-6 that the present invention, by doping metal ions of elements A, B and C, and at the same time, there is a synergistic effect between elements A, B and C, which helps to expand the interlayer spacing of the iron-manganese material and increase the sodium ion diffusion rate, so as to obtain a manganese-rich iron-based sodium ion battery positive electrode material with high rate performance.

[0102] (2) It can be seen from Examples 1 and 4 that the present invention can further expand the interlayer spacing of the positive electrode material and improve the rate performance by regulating the doping amount of the doping element. When the doping amount of the doping element is low, less doping elements enter the matrix, and the further expansion of the interlayer spacing is limited; when the doping amount of the doping element is high, the doping position is limited, the matrix is ​​not enough to accommodate more doping elements, and the further expansion of the interlayer spacing is also limited.

[0103] (3) It can be seen from Examples 1 and 5 that the doping ratio of the doping elements of the present invention has a preferred range. When the doping amounts of the three elements are within the preferred range, the interlayer spacing is further expanded and the rate performance is further improved. When the doping ratio is large or small, the repulsive force between the oxygen in the sodium layer and the supporting force of the doping element on the sodium layer cannot reach the optimal balance, so the interlayer spacing cannot be expanded most effectively.

[0104] (4) It can be seen from Examples 1 and 6-9 that the present invention further controls the sintering temperature and sintering time to prepare the positive electrode material, the interlayer spacing is not much different, and the rate performance is further improved. When the sintering time becomes longer or the temperature rises, oxygen-deficient compounds will be formed, resulting in the inability of the doping elements to function; on the other hand, too high a temperature will reduce the specific surface area of ​​the material, which is not conducive to the release and embedding of sodium ions; this will lead to a decrease in the rate performance of the material. When the sintering time becomes shorter or the temperature decreases, the inadequate reaction will cause the doping elements to be unable to fully enter the material, which will lead to a decrease in the rate performance of the material.

[0105] In summary, the present invention dopes large-particle metal ions into the manganese-rich iron-based sodium ion battery positive electrode material. These ions do not participate in the electrochemical reaction, but help to expand the interlayer spacing of the iron-manganese material and help to increase the sodium ion diffusion rate, so as to obtain a manganese-rich iron-based sodium ion battery positive electrode material with high rate performance.

[0106] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A low-cost manganese-rich iron-based sodium ion battery cathode material, characterized in that: The chemical general formula of the positive electrode material is Na u Fe 1-x Mn x M y O2, where 0.98 < u ≤ 1.05, 0.5 ≤ x ≤ 0.75, 0.03 ≤ y ≤ 0.2, the doping element M includes element A, element B and element C, wherein element A includes Y and / or La, element B includes Sr, and element C includes any one or a combination of at least two of Cd, K, Ca or Ba. The mass ratio of the element A, the element B and the element C is (0.5-2):(1-2):1; The interlayer spacing d of the positive electrode material satisfies 5.45Å≤d≤5.55Å.

2. A method for preparing the positive electrode material as claimed in claim 1, characterized in that: The preparation method comprises the following steps: Mixing an iron-manganese source, a sodium source and a dopant, and sintering to obtain the positive electrode material; The dopant includes a doping element M, M includes an A element, a B element and a C element, wherein the A element includes Y and / or La, the B element includes Sr, and the C element includes any one of Cd, K, Ca or Ba or a combination of at least two thereof.

3. The preparation method according to claim 2, characterized in that: The iron-manganese source includes any one of an iron-manganese hydroxide precursor, an iron-manganese oxide or an iron-manganese carbonate, or a combination of at least two thereof.

4. The preparation method according to claim 2, characterized in that: The mass ratio of the A element, the B element and the C element is (0.5-2):(1-2):

1.

5. The preparation method according to claim 4, characterized in that: The A element includes Y, the B element includes Sr, and the C element includes Cd.

6. The preparation method according to claim 2, characterized in that: The sintering temperature is 940-1200°C.

7. The preparation method according to claim 2, characterized in that: The sintering time is 10-14h.

8. The preparation method according to claim 2, characterized in that: The sintering atmosphere includes an oxygen-containing atmosphere.

9. The preparation method according to claim 2, characterized in that: The heating rate of the sintering is 4-5 min / °C, and the cooling rate of the sintering is 3-5 min / °C.

10. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode material according to claim 1, or the positive electrode material prepared by the preparation method according to any one of claims 2 to 9.