Hard carbon negative electrode sheet, method for preparing hard carbon negative electrode sheet and battery
By coating carboxylate-metal hydroxide on the second negative electrode coating of the hard carbon negative electrode sheet, the problem of forming sodium dendrites in the hard carbon negative electrode material in the sodium ion battery is solved, and the battery performance is achieved Improvement and safety performance enhancement.
Patent Information
- Application Number
- CN202411188162.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-28
AI Technical Summary
The hard carbon anode material in existing sodium ion batteries is prone to form sodium dendrites during charging and discharging, resulting in reduced battery performance and safety hazards.
Carboxylic acid ester-metal hydroxide is coated on the second negative electrode coating of the hard carbon negative electrode sheet, and the condensation reaction with the precipitated metal dendrites is inhibited to continue growing and the occurrence of side reactions is reduced.
It effectively inhibits the formation and growth of metal dendrites, and improves the cycle life, magnification characteristics, Coulomb efficiency and safety performance of the battery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to a hard carbon negative electrode sheet, a method for preparing the hard carbon negative electrode sheet, and a battery. Background Art
[0002] In recent years, carbon has been widely used as the negative electrode material of sodium ion batteries, especially hard carbon materials. Hard carbon materials have high specific capacity, so the prepared batteries have high sodium storage capacity. Hard carbon has small volume change during charge and discharge, so the prepared batteries have excellent cycle stability. Due to factors such as uneven distribution of sodium ions in the battery cycle, the capacity ratio of the negative electrode to the positive electrode in the sodium ion battery is not designed reasonably, affected by high and low temperatures, repeated electrode peeling, easy deposition, and the complex and diverse structure of hard carbon. The sodium storage sites are not easy to be fully exposed and utilized during the actual charge and discharge process, resulting in insufficient sodium embedding sites in the hard carbon negative electrode, resulting in sodium ion redundancy, causing the formation of sodium dendrites on the negative electrode surface. On the one hand, the formation of dendrites increases the chance of contact between metallic sodium and electrolyte, leading to the continuous occurrence of side reactions and continuous consumption of electrolyte, aggravating the formation of sodium dendrites and dead sodium, causing the volume expansion of the metallic sodium electrode, and making the battery cycle, rate characteristics, coulomb efficiency and other performance deteriorate. On the other hand, sodium dendrites will also pierce the diaphragm and reach the positive electrode of the battery, causing a series of safety hazards such as battery short circuit and thermal runaway.
[0003] Therefore, it is urgent to develop a hard carbon negative electrode sheet that can inhibit metal dendrites, thereby improving the electrochemical performance of the battery. Summary of the invention
[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a hard carbon negative electrode sheet, a method for preparing the hard carbon negative electrode sheet and a battery. In the hard carbon negative electrode sheet provided by the present invention, the carboxylate-metal hydroxide on the second negative electrode coating helps to inhibit metal dendrites, reduce the occurrence of side reactions, and improve the cycle life and safety performance of the battery.
[0005] In order to achieve the above-mentioned objectives, the first aspect of the present invention provides a hard carbon negative electrode sheet, which includes a current collector, a first negative electrode coating arranged on at least one side of the current collector surface, and a second negative electrode coating arranged on the side of the first negative electrode coating surface away from the current collector, wherein the first negative electrode coating includes hard carbon, and the second negative electrode coating includes a carboxylate-metal hydroxide.
[0006] Optionally, the mass ratio of the second negative electrode coating to the first negative electrode coating is 1:(2-5).
[0007] Optionally, based on the mass of the second negative electrode coating, the content of the carboxylate-metal hydroxide is 20-50 mass %.
[0008] Optionally, a ratio of the porosity of the first negative electrode coating to the porosity of the second negative electrode coating is 1:(1.1-2).
[0009] Optionally, a thickness ratio of the first negative electrode coating to the second negative electrode coating is (2-6):1.
[0010] Optionally, the porosity of the first negative electrode coating is 20%-30%.
[0011] Optionally, the porosity of the second negative electrode coating is 30%-40%.
[0012] Optionally, the thickness of the first negative electrode coating is 80µm-150µm.
[0013] Optionally, the thickness of the second negative electrode coating is 15µm-60µm.
[0014] Optionally, the first negative electrode coating further includes conductive carbon and a first binder.
[0015] Optionally, the second negative electrode coating further includes a second binder.
[0016] Optionally, the first binder and the second binder each independently include at least one of sodium hydroxymethyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, polyacrylic acid, polytetrafluoroethylene, polyethylene oxide, carboxypropyl methyl cellulose, polyvinylidene fluoride and hexafluoropropylene.
[0017] A second aspect of the present invention provides a method for preparing the hard carbon negative electrode sheet according to the first aspect, the method comprising:
[0018] (1) coating a first negative electrode slurry on the surface of the negative electrode current collector to obtain a first negative electrode coating;
[0019] (2) coating a second negative electrode slurry on the surface of the first negative electrode coating to obtain a second negative electrode coating;
[0020] The first negative electrode coating layer includes hard carbon, and the second negative electrode coating layer includes carboxylate-metal hydroxide.
[0021] Optionally, the method for preparing the first negative electrode slurry includes: mixing hard carbon, conductive carbon and a first binder to obtain the first negative electrode slurry.
[0022] Optionally, the preparation method of the second negative electrode slurry includes: reacting carboxylate, metal hydroxide and a first solution containing alkali to obtain carboxylate-metal hydroxide; mixing the carboxylate-metal hydroxide, a second binder and a solvent to obtain the second negative electrode slurry.
[0023] Optionally, the carboxylic acid ester includes at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate and ethyl propionate.
[0024] Optionally, the metal hydroxide includes at least one of aluminum hydroxide, copper hydroxide, cobalt hydroxide and zinc hydroxide.
[0025] Optionally, the alkali includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonia water and calcium hydroxide.
[0026] Optionally, the pH of the first solution is 8-11.
[0027] Optionally, the solvent is water.
[0028] Optionally, the reaction conditions include: temperature of 20°C-50°C, and time of 60min-180min.
[0029] A third aspect of the present invention provides a battery, comprising a positive electrode sheet, a separator and a hard carbon negative electrode sheet, wherein the hard carbon negative electrode sheet is the hard carbon negative electrode sheet described in the first aspect and / or the hard carbon negative electrode sheet obtained by the preparation method described in the second aspect.
[0030] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0031] (1) In the hard carbon negative electrode sheet provided by the present invention, the carboxylic acid ester on the second negative electrode coating can consume the metal dendrites precipitated during the cycle, inhibit the further deterioration of the metal dendrites, prevent the metal dendrites from piercing the diaphragm or reduce the occurrence of side reactions, thereby improving the cycle life, rate characteristics, coulombic efficiency and safety performance of the battery.
[0032] (2) In the hard carbon negative electrode sheet provided by the present invention, the carboxylate reacts with the metal hydroxide to form a carboxylate-metal hydroxide. The liquid carboxylate can be fixed on the surface of the hard carbon negative electrode sheet through the metal hydroxide, and the metal hydroxide is also uniformly distributed on the surface of the hard carbon negative electrode sheet by reacting with the carboxylate, which is more conducive to inhibiting metal dendrites and exerting better flame retardant properties.
[0033] (3) The mass ratio of the second negative electrode coating to the first negative electrode coating, the porosity ratio of the second negative electrode coating to the first negative electrode coating, and the thickness ratio of the second negative electrode coating to the first negative electrode coating in the hard carbon negative electrode sheet provided by the present invention work synergistically, so that the precipitation sites of metal ions in the positive electrode sheet and the receiving sites of metal ions in the hard carbon negative electrode sheet present a certain proportional relationship, and the carboxylate-metal hydroxide and free carboxylate groups in the second negative electrode coating can further consume excess metal dendrites, thereby inhibiting metal dendrites and improving the cycle performance of the battery.
[0034] The endpoints and any values of the range disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. DETAILED DESCRIPTION
[0035] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0036] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0037] A first aspect of the present invention provides a hard carbon negative electrode sheet, which includes a current collector, a first negative electrode coating arranged on at least one side of the current collector surface, and a second negative electrode coating arranged on the surface of the first negative electrode coating away from the current collector, wherein the first negative electrode coating includes hard carbon, and the second negative electrode coating includes a carboxylate-metal hydroxide.
[0038] In the present invention, the material of the current collector is not particularly limited.
[0039] In some embodiments, the first negative electrode coating further includes conductive carbon and a first binder.
[0040] The second negative electrode coating is disposed on the surface of the first negative electrode coating, and the second negative electrode coating comprises carboxylate-metal hydroxide.
[0041] Due to the unreasonable design of the capacity ratio of the negative electrode to the positive electrode during the battery cycle, or the influence of high and low temperatures, repeated electrode peeling and other factors, when the negative electrode capacity is insufficient to accommodate all the metal ions released from the positive electrode, the redundant metal ions will be deposited on the negative electrode surface to form metal dendrites. The carboxylic acid ester contained in the second negative electrode coating can undergo a condensation reaction with the metal dendrites, thereby avoiding further metal precipitation, helping to inhibit metal dendrites and preventing them from piercing the diaphragm.
[0042] In some embodiments, when the deintercalated metal ions are sodium ions, the carboxylate in the second negative electrode coating can undergo a spontaneous condensation reaction with the sodium dendrites, thereby reducing the sodium dendrites.
[0043] As used herein, the term "carboxylate-metal hydroxide" refers to a compound obtained by the reaction of a carboxylate with a metal hydroxide. The carboxylate and the metal hydroxide can undergo an addition reaction under alkaline solution conditions, wherein the carboxylate block reacts with the hydroxyl block of the metal hydroxide to obtain the carboxylate-metal hydroxide.
[0044] In some embodiments, the second negative electrode coating contains free carboxylate or metal hydroxide in addition to carboxylate-metal hydroxide, and the free carboxylate or metal hydroxide refers to the reaction raw material that does not participate in the addition reaction when the reaction raw material is excessive.
[0045] The carboxylate-metal hydroxide or free carboxylate contained in the second negative electrode coating can react with the metal dendrites on the hard carbon negative electrode sheet to condense, reduce the metal precipitation caused by high and low temperature charging and battery size, and avoid the metal precipitation caused by insufficient design N / P ratio, which is beneficial to reduce the precipitation of metal dendrites, inhibit the further growth of metal dendrites, reduce the occurrence of side reactions, and improve the cycle performance of the battery. At the same time, carboxylate-metal hydroxide also has good flame retardant properties, which can delay or prevent the risk of thermal runaway of the battery cell.
[0046] In some embodiments, the mass ratio of the second negative electrode coating to the first negative electrode coating is 1: (2-5), for example, it can be 1: 2, 1: 3, 1: 4 and 1: 5. When the mass ratio of the second negative electrode coating to the first negative electrode coating meets the above range, the precipitation sites of metal ions in the positive electrode sheet and the receiving sites of metal ions in the hard carbon negative electrode sheet can meet a certain relationship, and the carboxylate-metal hydroxide and free carboxylate groups in the second negative electrode coating can further consume metal dendrites, which are caused by excessive metal due to design or low temperature. It is also beneficial to inhibit the growth of metal dendrites and improve the cycle performance of the battery. When the mass ratio of the first negative electrode coating to the second negative electrode coating is greater than 5, the carboxylate groups contained in the second negative electrode coating are less, which are not enough to consume excessive metal dendrites. When the mass ratio of the first negative electrode coating to the second negative electrode coating is less than 2, the energy density of the battery is small.
[0047] In some embodiments, the porosity of the first negative electrode coating is less than the porosity of the second negative electrode coating. The porosity test method in the present invention is GB / T 33052-2016 "Determination of porosity of microporous functional films - hexadecane absorption method".
[0048] In some embodiments, the ratio of the porosity of the first negative electrode coating to the porosity of the second negative electrode coating is 1:(1.1-2), for example, it can be 1:1.5, 1:2, 2:3, 3:4, 3:5, 4:5 and 5:6. The porosity of the first negative electrode coating is less than the porosity of the second negative electrode, which is beneficial to improving the deintercalation ability of metal ions, so that the precipitation sites of metal ions in the positive electrode sheet and the receiving sites of metal ions in the hard carbon negative electrode sheet present a certain proportional relationship, and is more conducive to the carboxylate-metal hydroxide and free carboxylate groups in the second negative electrode coating to better consume the metal dendrites caused by design or low temperature, thereby inhibiting metal dendrites. When the ratio of the porosity of the second negative electrode coating to the porosity of the first negative electrode coating is less than 1.1, the porosity of the second negative electrode coating is small, and the metal ions are not easy to be deintercalated, resulting in battery capacity attenuation. Too few metal ions are embedded and embedded, resulting in a great attenuation of battery capacity, affecting the battery cycle performance. When the ratio of the porosity of the second negative electrode coating to the porosity of the first negative electrode coating is greater than 2, the porosity of the second negative electrode coating is relatively large, which easily provides a favorable place for the side reaction of the electrolyte, resulting in the aggravation of the side reaction and the aggravation of the consumption of the positive electrode material, which is not conducive to the battery's electrical performance.
[0049] In some embodiments, the porosity of the first negative electrode coating is 20%-30%, for example, 20%, 22%, 24%, 26%, 28% and 30%.
[0050] In some embodiments, the porosity of the second negative electrode coating is 30%-40%, for example, 30%, 32%, 34%, 36%, 38% and 40%.
[0051] In some embodiments, the thickness ratio of the first negative electrode coating to the second negative electrode coating is (2-6):1, such as 2:1, 3:1, 4:1, 5:1 and 6:1. At this time, it is more conducive to the precipitation sites of metal ions in the positive electrode sheet and the receiving sites of metal ions in the hard carbon negative electrode sheet to present a certain proportional relationship, and it is more conducive to the carboxylate-metal hydroxide and free carboxylate groups in the second negative electrode coating to further consume the metal dendrites caused by design or low temperature, thereby inhibiting metal dendrites and improving the cycle performance of the battery. The thickness test method is to measure using a micrometer. When the thickness ratio of the first negative electrode coating to the second negative electrode coating is less than 2, the thickness of the first negative electrode coating is smaller, the thickness of the second negative electrode coating is larger, and the energy density of the battery is smaller, which affects the capacity of the battery cell and fails to reach the normal capacity design value. When the thickness ratio of the first negative electrode coating to the second negative electrode coating is greater than 6, the thickness of the first negative electrode coating is larger and the thickness of the second negative electrode coating is smaller. At this time, the energy density of the battery is larger, but the inhibition of metal dendrites is poor, and the safety performance of the battery is also poor, so that the overall electrical performance and safety of the battery cell cannot be further guaranteed and optimized, which is not conducive to the long cycle of the battery cell.
[0052] In some embodiments, the thickness of the first negative electrode coating is 80µm-150µm, such as 80µm, 100µm, 120µm, 130µm, 140µm and 150µm.
[0053] In some embodiments, the thickness of the second negative electrode coating is 15µm-60µm, such as 15µm, 20µm, 30µm, 40µm, 50µm and 60µm.
[0054] In some embodiments, the first negative electrode coating includes hard carbon, conductive carbon, and a first binder.
[0055] In some embodiments, the first negative electrode coating further includes a functional additive.
[0056] In some embodiments, based on the mass of the first negative electrode coating, the mass ratio of the hard carbon, the conductive carbon and the first binder is 100:(3-8):(4-8). For example, the mass ratio of the hard carbon to the conductive carbon is 100:3, 100:4, 100:5, 100:6, 100:7 and 100:8. For example, the mass ratio of the hard carbon to the first conductive agent is 100:4, 100:5, 100:6, 100:7 and 100:8.
[0057] In some embodiments, the conductive carbon includes at least one of conductive carbon black (SP), graphite flakes, carbon nanotubes, graphene, and vapor-grown carbon fibers.
[0058] In some embodiments, the first binder includes at least one of sodium hydroxymethyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, polyacrylic acid, polytetrafluoroethylene, polyethylene oxide, carboxypropyl methyl cellulose, polyvinylidene fluoride and hexafluoropropylene.
[0059] In the present invention, the second negative electrode coating layer includes carboxylate-metal hydroxide.
[0060] In some embodiments, based on the mass of the second negative electrode coating, the content of the carboxylate-metal hydroxide is 20-50% by mass, such as 20%, 25%, 30%, 35%, 40%, 45% and 50%. When the content of the carboxylate-metal hydroxide is 20-50% by mass, the carboxylate can better consume the metal dendrites on the hard carbon negative electrode sheet and inhibit the growth of metal dendrites. When the content of the carboxylate-metal hydroxide is greater than 50% by mass, the carboxylate and the metal undergo a self-condensation reaction, which not only consumes the metal dendrites on the hard carbon negative electrode sheet, but also excessively consumes the metal ions in the battery, thereby affecting the battery capacity and cycle life. When the content of the carboxylate-metal hydroxide is less than 20% by mass, the content of the carboxylate is relatively small, and the spontaneous condensation reaction between the carboxylate and the metal dendrites can only consume a small amount of metal dendrites, and the generated metal dendrites cannot be removed in time, so that the continued generation of metal dendrites cannot be well inhibited.
[0061] In some embodiments, the molar ratio of the carboxylate and metal hydroxide in the reaction of the carboxylate-metal hydroxide reaction raw materials is (1-6): 1. When the molar ratio of the carboxylate and metal hydroxide in the reaction of the reaction raw materials is greater than 6, the carboxylate is excessive, and the content of carboxylate-metal hydroxide in the reaction product is small. At this time, the ability of the hard carbon negative electrode sheet to inhibit metal dendrites is weakened to a certain extent, and due to the small amount of metal hydroxide, the flame retardant performance of the carboxylate-metal hydroxide is limited, so the safety performance of the hard carbon negative electrode sheet is poor. When the molar ratio of the carboxylate and metal hydroxide in the reaction of the reaction raw materials is less than 1, the metal hydroxide is excessive, and there is an excess of metal hydroxide in the reaction product. At this time, due to the reduction of the carboxylate content, the ability of the hard carbon negative electrode sheet to inhibit metal dendrites becomes poor.
[0062] In some embodiments, based on the mass of the second negative electrode coating, the content of the free carboxylate is 0-40% by mass. When the content of the free carboxylate is greater than 40% by mass, the content of carboxylate-metal hydroxide in the second negative electrode coating is small, the cycle performance of the battery is poor, and the safety performance of the battery is also poor.
[0063] In some embodiments, based on the mass of the second negative electrode coating, the content of the free carboxylate is 0-10% by mass. When the content of the free carboxylate is 0-10% by mass, the content of carboxylate-metal hydroxide in the second negative electrode coating is relatively high. When the content of carboxylate-metal hydroxide is relatively high, the carboxylate with a higher content in the carboxylate-metal hydroxide can react spontaneously with the metal better, and the metal hydroxide also has a better flame retardant effect and is more helpful in suppressing thermal runaway. Therefore, the carboxylate-metal hydroxide can better suppress metal dendrites and improve the safety performance of the battery. In some embodiments, based on the mass of the second negative electrode coating, the content of the second binder is 20%-40% by mass, for example, it can be 20%, 25%, 30%, 35% and 40% by mass.
[0064] In some embodiments, the carboxylate group in the carboxylate-metal hydroxide may be selected from at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate, and ethyl propionate.
[0065] In some embodiments, the metal hydroxide group in the carboxylate-metal hydroxide may be selected from at least one of aluminum hydroxide, copper hydroxide, cobalt hydroxide, and zinc hydroxide.
[0066] In some embodiments, the carboxylate-metal hydroxide can be at least one of ethyl acetate-aluminum hydroxide, ethyl acetate-copper hydroxide, methyl propionate-aluminum hydroxide, methyl propionate-copper hydroxide, propyl acetate-aluminum hydroxide, propyl acetate-copper hydroxide, ethyl formate-aluminum hydroxide, ethyl formate-copper hydroxide, propyl formate-aluminum hydroxide and propyl formate-copper hydroxide.
[0067] In some embodiments, the second negative electrode coating further includes a second binder.
[0068] In some embodiments, the second binder includes at least one of sodium hydroxymethyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, polyacrylic acid, polytetrafluoroethylene, polyethylene oxide, carboxypropyl methyl cellulose, polyvinylidene fluoride and hexafluoropropylene.
[0069] In some embodiments, the second binder includes sodium hydroxymethyl cellulose and styrene-butadiene rubber mixed in a mass ratio of (2-5):1, such as 2:1, 3:1, 4:1 and 5:1.
[0070] A second aspect of the present invention provides a method for preparing the hard carbon negative electrode sheet according to the first aspect, the method comprising:
[0071] (1) coating a first negative electrode slurry on the surface of the negative electrode current collector to obtain a first negative electrode coating;
[0072] (2) coating a second negative electrode slurry on the surface of the first negative electrode coating to obtain a second negative electrode coating;
[0073] The second negative electrode coating layer includes carboxylate-metal hydroxide.
[0074] In some embodiments, the method for preparing the first negative electrode slurry includes: mixing hard carbon, conductive carbon and a first binder to obtain the first negative electrode slurry.
[0075] The components and contents of the hard carbon, conductive carbon and the first binder described here please refer to the first aspect and will not be described in detail here.
[0076] In some embodiments, the preparation method of the second negative electrode slurry includes: reacting carboxylate, metal hydroxide and a first solution containing alkali to obtain carboxylate-metal hydroxide; mixing the carboxylate-metal hydroxide, a second binder and a solvent to obtain the second negative electrode slurry. The hydroxyl group in the carboxylate can react with the metal hydroxide under alkaline conditions, so that the liquid carboxylate can be stably loaded on the surface of the hard carbon negative electrode sheet, and the metal hydroxide can be evenly distributed on the surface of the hard carbon negative electrode sheet.
[0077] In some embodiments, the pH of the first solution is 8-11, such as 8, 9, 10 and 11. Here, the pH of the first solution refers to the pH of the first solution containing a base.
[0078] In some embodiments, the reaction conditions include: a temperature of 20°C-50°C, such as 20°C, 30°C, 35°C, 40°C, 45°C and 50°C, and a time of 60min-180min, such as 60min, 80min, 100min, 120min, 140min, 160min and 180min.
[0079] In some embodiments, the base includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonia and calcium hydroxide.
[0080] In some embodiments, the carboxylic acid ester includes at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate, and ethyl propionate.
[0081] In some embodiments, the metal hydroxide includes at least one of aluminum hydroxide, copper hydroxide, cobalt hydroxide, and zinc hydroxide.
[0082] In the present invention, the carboxylate-metal hydroxide, the second binder and the solvent are mixed to obtain the second negative electrode slurry.
[0083] In some embodiments, the mass ratio of the carboxylate-metal hydroxide to the second binder is 1:(1-3), such as 1:2, 1:3, 2:5, 3:4 and 3:5.
[0084] In some embodiments, the solvent is water.
[0085] In some embodiments, the second binder includes at least one of sodium carboxymethylcellulose (CMC), styrene-butadiene rubber, polyvinyl alcohol, polyacrylic acid, polytetrafluoroethylene, polyethylene oxide, carboxypropyl methylcellulose, polyvinylidene fluoride and hexafluoropropylene.
[0086] In some embodiments, the second binder includes sodium hydroxymethyl cellulose and styrene-butadiene rubber mixed in a mass ratio of (2-5):1, such as 2:1, 3:1, 4:1 and 5:1.
[0087] A third aspect of the present invention provides a battery, comprising a positive electrode sheet, a separator and a hard carbon negative electrode sheet, wherein the hard carbon negative electrode sheet is the hard carbon negative electrode sheet described in the first aspect and / or the hard carbon negative electrode sheet obtained by the preparation method of the second aspect.
[0088] The type of battery described in the present invention is not specifically limited, and can be a lithium ion battery, a sodium ion battery, a potassium ion battery, etc.
[0089] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0090] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0091] The present invention is described in detail below in conjunction with specific examples, which are used to understand but not to limit the present invention. In the following examples, 1 part represents 1 g.
[0092] Preparation Example
[0093] The following preparation examples prepare a material containing carboxylate-metal hydroxide in the second negative electrode slurry.
[0094] Preparation Example 1
[0095] Ethyl acetate and aluminum hydroxide in a molar ratio of 3:1 were placed in a potassium hydroxide solution with a pH of 10 and stirred evenly, the reaction temperature was 30° C., and the reaction time was 120 minutes to obtain a material A1 containing ethyl acetate-aluminum hydroxide. The content of ethyl acetate-aluminum hydroxide in A1 was 70%, the content of free ethyl acetate was 10%, and the rest was solvent.
[0096] Preparation Example 2
[0097] The method described in Preparation Example 1 was followed, except that the molar ratio of ethyl acetate to aluminum hydroxide was 6:1, to obtain material A2 containing ethyl acetate-aluminum hydroxide. The content of ethyl acetate-aluminum hydroxide in A2 was 60%, the content of free ethyl acetate was 20%, and the rest was solvent.
[0098] Preparation Example 3
[0099] The method described in Preparation Example 1 was followed, except that the molar ratio of ethyl acetate to aluminum hydroxide was 2:1, to obtain material A3 containing ethyl acetate-aluminum hydroxide. The content of ethyl acetate-aluminum hydroxide in A3 was 75%, the content of free ethyl acetate was 5%, and the rest was solvent.
[0100] Preparation Example 4
[0101] The method described in Preparation Example 1 was followed, except that the molar ratio of ethyl acetate to aluminum hydroxide was 4:1, to obtain material A4 containing ethyl acetate-aluminum hydroxide. The content of ethyl acetate-aluminum hydroxide in A3 was 65%, the content of free ethyl acetate was 15%, and the rest was solvent.
[0102] Preparation Example 5
[0103] The method described in Preparation Example 1 was followed, except that the molar ratio of ethyl acetate to aluminum hydroxide was 1:1, to obtain material A5 containing ethyl acetate-aluminum hydroxide. The content of ethyl acetate-aluminum hydroxide in A5 was 80%, the content of free ethyl acetate was 0%, and the rest was solvent.
[0104] Preparation Example 6
[0105] The method described in Preparation Example 1 was followed, except that the molar ratio of ethyl acetate to aluminum hydroxide was 1:2, to obtain material A6 containing ethyl acetate-aluminum hydroxide. The content of ethyl acetate-aluminum hydroxide in A6 was 70%, the content of free aluminum hydroxide was 10%, and the rest was solvent.
[0106] Preparation Example 7
[0107] The method described in Preparation Example 1 was followed, except that when the pH of the potassium hydroxide solution was 8, a material A7 containing ethyl acetate-aluminum hydroxide was obtained. The content of ethyl acetate-aluminum hydroxide in A7 was 70%, the content of free ethyl acetate was 10%, and the rest was solvent.
[0108] Preparation Example 8
[0109] The process described in Preparation Example 1 was followed, except that the pH of the potassium hydroxide solution was 13, to obtain material A8 containing ethyl acetate-aluminum hydroxide. The content of ethyl acetate-aluminum hydroxide in A8 was 70%, the content of free ethyl acetate was 10%, and the rest was solvent.
[0110] Example 1
[0111] This example is used to illustrate the preparation of the hard carbon negative electrode sheet of the present invention.
[0112] (1) Take 91 parts of hard carbon, 3 parts of SP, and 6 parts of CMC, stir and mix the hard carbon, SP, and CMC for 15 minutes, then add an appropriate amount of deionized water and continue stirring for 25 minutes to obtain the first negative electrode slurry;
[0113] (2) Take 30 parts of CMC, 10 parts of styrene-butadiene rubber, and 15 parts of deionized water, stir, add 20 parts of material A1 obtained in Preparation Example 1 (based on the mass of ethyl acetate-aluminum hydroxide), and continue stirring for 120 minutes to obtain a second negative electrode slurry;
[0114] (3) A first negative electrode slurry is coated on an aluminum foil, and after drying, a first negative electrode coating is obtained. A second negative electrode slurry is coated on the side of the first negative electrode coating away from the aluminum foil, and after drying, a second negative electrode coating is obtained. The mass ratio of the second negative electrode coating to the first negative electrode coating is 1:4. The porosity of the first negative electrode coating is 30% and the thickness is 120µm; the porosity of the second negative electrode coating is 40% and the thickness is 30µm.
[0115] Example 2
[0116] This example is used to illustrate the preparation of hard carbon negative electrode sheets when the proportions of carboxylate-metal hydroxide in the material containing carboxylate-metal hydroxide obtained in the preparation example are different.
[0117] Example 2-1
[0118] The operation was carried out in accordance with the method described in Example 1, except that material A1 was replaced with the same mass fraction of material A2 obtained in Preparation Example 2, calculated on the mass of ethyl acetate-aluminum hydroxide.
[0119] Example 2-2
[0120] The operation was carried out in accordance with the method described in Example 1, except that material A1 was replaced by the same mass portion of material A3 obtained in Preparation Example 3 based on the mass of ethyl acetate-aluminum hydroxide.
[0121] Example 2-3
[0122] The operation was carried out in accordance with the method described in Example 1, except that material A1 was replaced by the same mass fraction of material A4 obtained in Preparation Example 4, calculated on the mass of ethyl acetate-aluminum hydroxide.
[0123] Embodiment 2-4
[0124] The operation was carried out in accordance with the method described in Example 1, except that material A1 was replaced by the same mass portion of material A5 obtained in Preparation Example 5, calculated on the mass of ethyl acetate-aluminum hydroxide.
[0125] Embodiment 2-5
[0126] The operation was carried out in accordance with the method described in Example 1, except that material A1 was replaced by the same mass fraction of material A6 obtained in Preparation Example 6, calculated on the mass of ethyl acetate-aluminum hydroxide.
[0127] Example 3
[0128] This example is used to illustrate the preparation of hard carbon negative electrode sheets at different pH values of potassium hydroxide solutions.
[0129] Example 3-1
[0130] The operation was carried out in accordance with the method described in Example 1, except that material A1 was replaced with the same mass portion of material A7 obtained in Preparation Example 7 based on the mass of ethyl acetate-aluminum hydroxide.
[0131] Example 3-2
[0132] The operation was carried out in accordance with the method described in Example 1, except that material A1 was replaced by the same mass portion of material A8 obtained in Preparation Example 8, calculated on the mass of ethyl acetate-aluminum hydroxide.
[0133] Example 4
[0134] This example is used to illustrate the preparation of a hard carbon negative electrode sheet when different portions of the material A1 obtained in Preparation Example 1 are added in step (2).
[0135] Example 4-1
[0136] The process described in Example 1 was followed, except that 5 parts of the material A1 obtained in Preparation Example 1 were added in step (2) based on the mass of ethyl acetate-aluminum hydroxide.
[0137] Example 4-2
[0138] The process described in Example 1 was followed, except that 40 parts of the material A1 obtained in Preparation Example 1 were added in step (2) based on the mass of ethyl acetate-aluminum hydroxide.
[0139] Example 5
[0140] This example is used to illustrate the preparation of a hard carbon negative electrode sheet when the thickness ratio of the second negative electrode coating layer to the first negative electrode coating layer is different.
[0141] Example 5-1
[0142] The method described in Example 1 was followed, except that the thickness of the second negative electrode coating was 20 μm.
[0143] Example 5-2
[0144] The method described in Example 1 was followed, except that the thickness of the second negative electrode coating was 60 μm.
[0145] Comparative Example 1
[0146] This comparative example is used to illustrate the preparation of a hard carbon negative electrode sheet when no second negative electrode coating is provided on the hard carbon negative electrode sheet.
[0147] The method described in Example 1 was followed, except that no second negative electrode coating was provided on the aluminum foil.
[0148] Comparative Example 2
[0149] This comparative example is used to illustrate the preparation of a hard carbon negative electrode sheet when the second slurry on the hard carbon negative electrode sheet does not contain carboxylate.
[0150] The process described in Example 1 was followed, except that the carboxylic acid ester in step (2) was replaced by the same amount of aluminum hydroxide.
[0151] Comparative Example 3
[0152] This comparative example is used to illustrate the preparation of a hard carbon negative electrode sheet when the second slurry on the hard carbon negative electrode sheet does not contain metal hydroxide.
[0153] The process described in Example 1 was followed, except that the aluminum hydroxide in step (2) was replaced by the same mass fraction of carboxylic acid ester.
[0154] Comparative Example 4
[0155] This comparative example is used to illustrate the preparation of a hard carbon negative electrode sheet when the aluminum hydroxide in the second slurry on the hard carbon negative electrode sheet does not react with the carboxylic acid ester.
[0156] The procedure described in Example 1 was followed, except that ethyl acetate was directly mixed with aluminum hydroxide without adding potassium hydroxide solution.
[0157] Test Case
[0158] Preparation of positive electrode sheet: weigh 93 parts of sodium nickel cobalt manganese oxide, 3 parts of SP, 4 parts of PVDF, and 35 parts of NMP, stir and mix lithium iron phosphate, SP, PVDF and functional additives for 15 minutes, then add NMP to make slurry, continue stirring for 25 minutes, and use it for coating after stirring, wind it into a battery cell, assemble it into a battery, coat it on aluminum foil, blow dry it at 100°C, and cold press and cut it into positive electrode sheets;
[0159] Battery preparation: The positive electrode sheet, the separator, and the hard carbon negative electrode sheet obtained in the embodiment are wound into a roll core, wherein the separator completely covers the positive electrode sheet and the hard carbon negative electrode sheet, and then the roll core is placed in a metal shell or wrapped with an aluminum-plastic film and then injected with electrolyte. Finally, a sodium ion battery is made through processes such as standing, formation, and capacity separation;
[0160] (1) Cycle test: At 25°C, charge the battery at 0.5C constant current and constant voltage to 4.0V, with a cut-off condition of 0.05C; let it stand for 60 minutes and then discharge it at 0.5C to 2.0V. Continue the above process until the capacity decays to 80% of the initial test capacity, and record the cycle number.
[0161] (2) 2000 cycles capacity retention rate (%):
[0162] 1. Take the battery after capacity division and charge it to 4.25V with a constant current of 1C, and then charge it to I≤0.05C with a constant voltage of 4.25V; 2. After standing for 5 minutes, discharge the battery to 2.8V with a constant current of 1C to obtain the discharge capacity C1; 3. Stand for 30 minutes. Repeat steps 1-3 1999 times to obtain the discharge capacity C2000; the capacity retention rate after 2000 cycles is calculated as (C2000) / (C1)*100%.
[0163] (3) Thermal runaway test: Use a flat or rod-shaped heating device, and its surface should be covered with ceramic, metal or insulating layer, so that the heating power of the heating device is greater than 1000W. The heating device should be in direct contact with the battery. The size of the heating device should be close to the size of the heated surface of the battery cell and should not be larger than the heated surface of the battery cell. Charge at a constant current of 220A until overcharged, and start the heating device at the same time and continue to heat the test object at its maximum power. When thermal runaway occurs or the temperature at the monitoring point reaches 350℃, ensure that the battery cell failure detection is carried out for 30 minutes, stop triggering and turn off the heating device (detect fire, smoke, etc.).
[0164]
[0165] In Preparation Examples 1 to 7, materials containing ethyl acetate-aluminum hydroxide are obtained by reacting ethyl acetate and aluminum hydroxide in different molar ratios, and the content of ethyl acetate-aluminum hydroxide in the materials obtained in different Preparation Examples is different. In Examples 1 to 2-5, the materials of Preparation Examples 1 to 7 are taken in the same mass parts based on the mass of ethyl acetate-aluminum hydroxide, so the mass of ethyl acetate-aluminum hydroxide crosslinked products in Examples 1 to 2-5 is the same, but the content of free ethyl acetate or free aluminum hydroxide is different. Ethyl acetate has an inhibitory effect on metal dendrites, and too much or too little free ethyl acetate is not conducive to improving the battery cycle performance.
[0166] In the embodiment, a material containing ethyl acetate-aluminum hydroxide is obtained by reacting ethyl acetate and aluminum hydroxide in different molar ratios, or by adding different mass portions of ethyl acetate-aluminum hydroxide, or by making the thickness ratio of the second negative electrode coating to the first negative electrode coating different, to obtain a hard carbon negative electrode sheet containing different mass of ethyl acetate-aluminum hydroxide, different mass of free ethyl acetate or free aluminum hydroxide.
[0167] The number of cycles and the 2000-cycle capacity retention rate of the embodiment are much higher than those of the comparative example, that is, the second negative electrode coating of the scheme of the present invention contains carboxylate-metal hydroxide, which is indeed helpful to inhibit metal dendrites, reduce the occurrence of side reactions, and can improve the cycle life and capacity retention rate of the battery. In addition, in this embodiment, the battery cell was subjected to a thermal runaway test, and the battery cell did not catch fire, that is, the second negative electrode coating containing carboxylate-metal hydroxide is indeed helpful to improve the safety performance of the battery. In Comparative Example 1, since there is no second negative electrode coating, the inhibitory effect on metal dendrites is poor, and the safety performance of the battery is also poor. Therefore, the number of cycles and the 2000-cycle capacity retention rate in Comparative Example 1 are small, and the battery cell catches fire during the thermal runaway test. Comparative Example 2 does not contain ethyl acetate, so the inhibitory effect on metal dendrites is poor, but since it contains aluminum hydroxide, the safety performance of the battery is improved to a certain extent. Comparative Example 3 contains ethyl acetate but does not contain aluminum hydroxide, and the number of cycles and 2000-cycle capacity retention rate of the battery are improved to a certain extent compared with Comparative Example 1, but the effect is poor compared with Example 1. Comparative Example 4 contains both ethyl acetate and aluminum hydroxide, but the two do not undergo an addition reaction. The number of battery cycles and the 2000-cycle capacity retention rate are improved to a certain extent compared with Comparative Example 1, but the effect is worse than that of Example 1, that is, the carboxylate in the second negative electrode coating and the metal hydroxide can only generate a carboxylate-metal hydroxide cross-linked product, which is more helpful to inhibit metal dendrites, reduce the occurrence of side reactions, and improve the cycle life and safety performance of the battery.
[0168] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0169] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A hard carbon negative electrode sheet, characterized in that: The hard carbon negative electrode sheet comprises a current collector, a first negative electrode coating disposed on at least one side of the current collector surface, and a second negative electrode coating disposed on the first negative electrode coating surface away from the current collector, wherein the first negative electrode coating comprises hard carbon, and the second negative electrode coating comprises carboxylate-metal hydroxide; The carboxylate-metal hydroxide is a compound obtained by reacting a carboxylate with a metal hydroxide under alkaline solution conditions; The second negative electrode coating further includes free carboxylate or free metal hydroxide; The carboxylic acid ester includes at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate and ethyl propionate; The metal hydroxide includes at least one of aluminum hydroxide, copper hydroxide, cobalt hydroxide and zinc hydroxide.
2. The hard carbon negative electrode sheet according to claim 1, characterized in that: The mass ratio of the second negative electrode coating to the first negative electrode coating is 1:(2-5); and / or, Based on the mass of the second negative electrode coating, the content of the carboxylate-metal hydroxide is 20-50 mass %.
3. The hard carbon negative electrode sheet according to claim 1, characterized in that: The ratio of the porosity of the first negative electrode coating to the porosity of the second negative electrode coating is 1:(1.1-2); and / or, The thickness ratio of the first negative electrode coating to the second negative electrode coating is (2-6):
1.
4. The hard carbon negative electrode sheet according to claim 1, characterized in that: The porosity of the first negative electrode coating is 20%-30%; and / or, The porosity of the second negative electrode coating is 30%-40%; and / or, The thickness of the first negative electrode coating is 80 μm-150 μm; and / or, The thickness of the second negative electrode coating is 15µm-60µm.
5. The hard carbon negative electrode sheet according to claim 1, characterized in that: The first negative electrode coating further includes conductive carbon and a first binder; and / or, the second negative electrode coating further comprises a second binder; and / or, The first binder and the second binder each independently include at least one of sodium hydroxymethyl cellulose, styrene-butadiene rubber, polyvinyl alcohol, polyacrylic acid, polytetrafluoroethylene, polyethylene oxide, carboxypropyl methyl cellulose, polyvinylidene fluoride and hexafluoropropylene.
6. A method for preparing the hard carbon negative electrode sheet according to any one of claims 1 to 5, characterized in that: The method comprises: (1) coating a first negative electrode slurry on the surface of the negative electrode current collector to obtain a first negative electrode coating; (2) coating a second negative electrode slurry on the surface of the first negative electrode coating to obtain a second negative electrode coating; The first negative electrode coating layer includes hard carbon, and the second negative electrode coating layer includes carboxylate-metal hydroxide.
7. The method according to claim 6, characterized in that: The method for preparing the first negative electrode slurry comprises: mixing hard carbon, conductive carbon and a first binder to obtain the first negative electrode slurry; and / or, The preparation method of the second negative electrode slurry includes: reacting carboxylate, metal hydroxide and a first solution containing alkali to obtain carboxylate-metal hydroxide; mixing the carboxylate-metal hydroxide, a second binder and a solvent to obtain the second negative electrode slurry.
8. The method according to claim 7, characterized in that: The carboxylic acid ester comprises at least one of ethyl acetate, propyl acetate, ethyl formate, propyl formate, methyl propionate and ethyl propionate; and / or, The metal hydroxide includes at least one of aluminum hydroxide, copper hydroxide, cobalt hydroxide and zinc hydroxide.
9. The method according to claim 8, characterized in that The alkali includes at least one of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonia water and calcium hydroxide; and / or, The pH of the first solution is 8-11; and / or, The solvent is water; and / or, The reaction conditions include: temperature of 20°C-50°C, and time of 60min-180min.
10. A battery, characterized in that: The battery comprises a positive electrode sheet, a separator and a hard carbon negative electrode sheet, wherein the hard carbon negative electrode sheet is the hard carbon negative electrode sheet according to any one of claims 1 to 5 and / or the hard carbon negative electrode sheet obtained by any one of the preparation methods according to claims 6 to 9.
Citation Information
Patent Citations
Composite negative electrode material, preparation method of composite negative electrode material, negative electrode piece and battery
CN109994710A
Pole piece, secondary battery and electric device comprising same
CN115939307A
Pre-magnesium-silicon-oxygen negative electrode material, preparation method thereof and secondary battery
CN116864653A
Electrode protective film forming agent
JP2012256515A
Battery pack
US20100310911A1