Absorbable biological membrane and manufacturing method thereof

By treating type I recombinant collagen with specific short amino acid sequence repeats at low temperature and performing irradiation cross-linking to form a polymer, the problem of short degradation time of the recombinant collagen film is solved and it is possible to maintain flexibility and suitability for dental applications. degradation time, suitable for dental materials.

CN118718121APending Publication Date: 2024-10-01SHAANXI GIANT BIOTECHNOLOGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410092488.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-01-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The degradation time of existing recombinant collagen membranes is short, and increasing the degradation time can easily lead to a decrease in flexibility, which limits their use in dental applications.

Method used

By pre-cooling and irradiating cross-linking the type I recombinant collagen with a specific short amino acid sequence repeated 52 times at low temperatures to form a polymer, it can obtain strong resistance to degradation and maintain flexibility at low cross-linking degrees. And control the degradation time within 6-12 weeks.

Benefits of technology

An oral collagen membrane with low potential immunogenicity and low risk of viral infection, and a degradation time that meets the needs of periodontal tissue regeneration has been achieved. It maintains flexibility and an appropriate degradation time, and is suitable for dental materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004678268370000071
    Figure BDA0004678268370000071
  • Figure BDA0004678268370000081
    Figure BDA0004678268370000081
  • Figure HDA0004678268810000011
    Figure HDA0004678268810000011
Patent Text Reader

Abstract

The invention relates to an absorbable biological membrane and a manufacturing method thereof. The manufacturing method of the absorbable biological membrane comprises the following steps: pre-cooling 2-6 wt% of a collagen aqueous solution at a temperature of 2-5 DEG C for more than 2 hours; immediately placing the pre-cooled collagen aqueous solution at the temperature of 2-8 DEG C, and carrying out irradiation crosslinking; the irradiation dose of the irradiation crosslinking is 40 to 80 kGy; and carrying out freeze drying on the collagen aqueous solution after irradiation crosslinking so as to obtain the absorbable biological membrane. Wherein the amino acid sequence of the collagen is an amino acid sequence obtained by repeating a short amino acid sequence as shown in SEQ ID NO: 1 for 52 times. The degradation time of the absorbable biological membrane reaches or exceeds the time required by periodontal tissue regeneration; and the collagen membrane is flexible in texture, has the capability of maintaining space, and can be clinically used as an oral cavity collagen membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of biomaterials, and specifically relates to a recombinant collagen membrane that can be absorbed by the body and a method for manufacturing the same. Background Art

[0002] The barrier membrane acts as a mechanical barrier between soft tissue and defective bone tissue during guided tissue regeneration (GTR) or guided bone regeneration (GBR) surgery. It can maintain the defect space and block the growth of rapidly proliferating epithelial cells and fibroblasts, ensuring that the slower proliferating osteoblasts grow dominantly to form new bone tissue, thereby regenerating periodontal defect tissue. It is reported that about 40% of patients need guided bone regeneration when undergoing implant restoration. Among them, the most widely used is oral collagen membrane.

[0003] Oral collagen membrane refers to oral membrane materials with collagen as the main component, generally including purified collagen membrane, recombinant collagen membrane and decellularized matrix membrane. Purified collagen membrane refers to a membrane product prepared by physical or chemical cross-linking of collagen extracted from animal tissues; recombinant collagen membrane refers to a membrane product prepared by physical or chemical cross-linking of collagen prepared by genetic engineering technology; decellularized matrix membrane is mainly a membrane with extracellular matrix as the main component obtained by removing the cellular components of tissues / organs by chemical and / or physical methods while retaining its tissue structure. Among them, in terms of degradation time, decellularized matrix membrane is the longest, followed by purified collagen membrane, and recombinant collagen membrane is the shortest.

[0004] The degradation time of oral collagen membrane varies depending on the material and manufacturing process. The ideal degradation rate of oral collagen membrane should match the rate of tissue reconstruction. Different degradation times are required depending on the target regeneration tissue. Literature reports that periodontal tissue regeneration requires 6-8 weeks, so the degradation time of oral collagen membrane as a support material is preferably 6-12 weeks. Compared with decellularized matrix membrane and purified collagen membrane, recombinant collagen membrane has the advantages of potential immunogenicity and low risk of viral infection, but its short degradation time limits its application as a dental support material.

[0005] In order to prolong the degradation time of recombinant collagen membrane, technicians can use two methods: one is to increase the content of recombinant collagen, and the other is to cross-link. However, no matter which method is used, there is a limit. Increasing the content of recombinant collagen or the degree of cross-linking beyond the limit will cause the recombinant collagen membrane to become brittle. As an oral collagen membrane, it must maintain a certain degree of flexibility to facilitate clinical use.

[0006] Therefore, for oral collagen membranes, how to maintain their flexibility while controlling their degradation within the expected 6-12 weeks is a technical challenge that needs to be solved. Summary of the invention

[0007] In view of the technical problems existing in the prior art, the object of the present invention is to provide an oral collagen membrane with low potential immunogenicity and virus transmission risk, a degradation time controlled within 6-12 weeks and maintaining flexibility.

[0008] The inventors conducted in-depth research to solve the above technical problems, and found that the type I recombinant collagen obtained by repeating the short amino acid sequence shown in SEQ ID NO: 1 (G AP GAPG SQ GAPGLQ) 52 times can self-assemble to a certain extent at low temperature (2-5°C) to form a polymer, and the formation of the polymer enables the type I recombinant collagen to obtain a strong anti-degradation ability at a low cross-linking degree without significantly making the recombinant collagen film brittle. Based on the above findings, the inventors completed the present invention and obtained an oral collagen film with low potential immunogenicity and virus transmission risk, a degradation time controlled at 6-12 weeks, and maintained flexibility.

[0009] That is, the present invention includes:

[0010] 1. A method for producing an absorbable biofilm, comprising:

[0011] Step A: precooling a 2-6 wt% collagen aqueous solution to a temperature of 2-5° C. and maintaining the temperature for more than 2 hours;

[0012] Step B: Immediately placing the pre-cooled collagen aqueous solution at 2-8° C. and irradiating and cross-linking the solution; the irradiation dose for the irradiation and cross-linking is 40-80 kGy;

[0013] Step C: freeze-drying the irradiated cross-linked collagen aqueous solution to obtain the absorbable biofilm;

[0014] The amino acid sequence of the collagen is an amino acid sequence obtained by repeating the short amino acid sequence represented by SEQ ID NO: 1 (GAPGAPG SQ GAP GL Q) 52 times.

[0015] 2. The manufacturing method according to item 1, wherein the radiation source for the radiation cross-linking is selected from ultraviolet rays, gamma rays, X-rays, neutron beams, particle beams or electron beams.

[0016] 3. The production method according to item 1, wherein in step A, the 2 to 6 wt % collagen aqueous solution is pre-cooled to a temperature of 2 to 5° C. and maintained for more than 4 hours.

[0017] 4. According to the manufacturing method described in item 1, it also includes step D between step A and step B: rapidly freezing the pre-cooled collagen aqueous solution to fix its shape.

[0018] 5. The production method according to item 1, further comprising the step of cutting the absorbable biofilm obtained after freeze-drying into a specified size and sterilizing it.

[0019] 6. The production method according to item 1, wherein the in vivo degradation time of the absorbable biofilm is 6 to 12 weeks.

[0020] 7. The manufacturing method according to item 1, wherein the absorbable biomembrane is an oral collagen membrane.

[0021] 8. An absorbable biofilm produced by the production method according to any one of items 1 to 7.

[0022] 9. Use of the absorbable biofilm obtained by the manufacturing method described in any one of items 1 to 7 in the preparation of dental materials, wherein the dental material is an oral collagen membrane, which is used for guided bone regeneration while performing oral dental implants, guided bone regeneration around implants during immediate implantation after tooth extraction, guided bone regeneration around implants during delayed implantation after tooth extraction, guided bone regeneration in bone fracture-type bone defects, local ridge augmentation, alveolar ridge augmentation, root resection, oral cyst resection and filling of bone defect areas after residual root extraction, and periodontal bone defects.

[0023] Based on the present invention, the recombinant collagen can be obtained through genetic engineering expression, which effectively reduces the potential immunogenicity and viral transmission risk of the product; the degradation time of the prepared absorbable biofilm reaches or exceeds the time required for periodontal tissue regeneration; and the texture is flexible and has the ability to maintain space, and can be used clinically as an oral collagen membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1A These are photos of the absorbable biofilm of Example 1 implanted subcutaneously in New Zealand rabbits for 6 weeks.

[0025] Figure 1B These are photos of the absorbable biofilm of Example 1 implanted subcutaneously in New Zealand rabbits for 7 weeks.

[0026] Figure 2A These are photos of the absorbable biofilm of Example 2 implanted subcutaneously in New Zealand rabbits for 5 weeks.

[0027] Figure 2B These are photos of the absorbable biofilm of Example 2 implanted subcutaneously in New Zealand rabbits for 6 weeks.

[0028] Figure 3AThese are photos of the absorbable biofilm of Example 3 implanted subcutaneously in New Zealand rabbits for 5 weeks.

[0029] Figure 3B These are photos of the absorbable biofilm of Example 3 implanted subcutaneously in New Zealand rabbits for 6 weeks.

[0030] Figure 4A These are photos of the absorbable biofilm of Example 4 implanted subcutaneously in New Zealand rabbits for 10 weeks.

[0031] Figure 4B These are photos of the absorbable biofilm of Example 4 implanted subcutaneously in New Zealand rabbits for 11 weeks.

[0032] Figure 5A These are photos of the absorbable biofilm of Comparative Example 1 implanted subcutaneously in New Zealand rabbits for 3 weeks.

[0033] Figure 5B These are photos of the absorbable biofilm of Comparative Example 1 implanted subcutaneously in New Zealand rabbits for 4 weeks.

[0034] Fig. 6A These are photos of the absorbable biofilm of Comparative Example 3 implanted subcutaneously in New Zealand rabbits for 4 weeks.

[0035] Figure 6B This is a photograph of the absorbable biofilm of Comparative Example 3 implanted subcutaneously in New Zealand rabbits for 5 weeks.

[0036] Fig. 7A These are photos of the absorbable biofilm of Comparative Example 4 implanted subcutaneously in New Zealand rabbits for 4 weeks.

[0037] Figure 7B This is a photograph of the absorbable biofilm of Comparative Example 4 implanted subcutaneously in New Zealand rabbits for 5 weeks.

[0038] Fig. 8A This is a photograph of the absorbable biofilm of Comparative Example 5 implanted subcutaneously in New Zealand rabbits for 4 weeks.

[0039] Figure 8B This is a photograph of the absorbable biofilm of Comparative Example 5 implanted subcutaneously in New Zealand rabbits for 5 weeks.

[0040] Fig. 9 This is a transmission electron microscope photograph of the collagen solution in Example 1 taken immediately after precooling.

[0041] Fig.10 This is a transmission electron microscope photo of the collagen solution in Comparative Example 4 taken immediately after precooling. DETAILED DESCRIPTION

[0042] The present application is further described below in conjunction with examples. It should be understood that the examples are only used to further describe and illustrate the present application and are not used to limit the present application.

[0043] According to Example 2 of Chinese patent application publication CN115947828A, type I recombinant collagen (ie, HLC protein as referred to in the above Chinese patent application publication) was prepared.

[0044] Example 1 Preparation of absorbable biofilm 1

[0045] Accurately weigh 4 g of type I recombinant collagen and 96 g of water for injection, and fully dissolve them to obtain a 4% by weight recombinant collagen solution.

[0046] The recombinant collagen solution was filled into a specific mold and precooled at 4°C for 4 hours.

[0047] The dosage was set to 60 kgy, and the pre-cooled recombinant collagen solution was cross-linked at 5±3°C using an electron accelerator.

[0048] The freeze-drying parameters were set and the freeze-drying of the cross-linked recombinant collagen solution was completed using a vacuum freeze dryer.

[0049] The freeze-dried recombinant collagen solution is pressed, cut and sterilized using relevant equipment to obtain absorbable biofilms of different sizes.

[0050] Example 2 Preparation of absorbable biofilm 2

[0051] An absorbable biomembrane was prepared as in Example 1, except that the concentration of type I recombinant collagen was 2% by weight, and the radiation cross-linking dose was 40 kgy, to prepare an absorbable biomembrane of Example 2, which is absorbable biomembrane 2 of the example.

[0052] Example 3 Preparation of absorbable biofilm 3

[0053] The absorbable biomembrane was prepared as in Example 1, except that the precooling temperature was 5° C. and maintained for 3 h, and the absorbable biomembrane of Example 3 was prepared, which is the absorbable biomembrane 3 of the example.

[0054] Example 4 Preparation of absorbable biofilm 4

[0055] An absorbable biomembrane was prepared as in Example 1, except that the concentration of type I recombinant collagen was 6% by weight, the precooling temperature was 2°C, maintained for 2 hours, and the irradiation cross-linking dose was 80 kgy. An absorbable biomembrane of Example 4 was prepared, which is the absorbable biomembrane 4 of the example.

[0056] Comparative Example 1

[0057] An absorbable biomembrane was prepared as in Example 1, except that the concentration of type I recombinant collagen was 1% by weight, and an absorbable biomembrane of Comparative Example 1 was prepared, which is absorbable biomembrane 1 of Comparative Example.

[0058] Comparative Example 2

[0059] An absorbable biomembrane was prepared as in Example 1, except that the concentration of type I recombinant collagen was 8% by weight, and an absorbable biomembrane of Comparative Example 2 was prepared, which is absorbable biomembrane 2 of Comparative Example.

[0060] Comparative Example 3

[0061] An absorbable biomembrane was prepared as in Example 1, except that the precooling temperature was 8° C., and an absorbable biomembrane of Comparative Example 3 was prepared, which was absorbable biomembrane 4 of Comparative Example.

[0062] Comparative Example 4

[0063] An absorbable biofilm was prepared as in Example 1, except that the holding time was 0.5 h, and an absorbable biofilm of Comparative Example 4 was prepared, which is absorbable biofilm 4 of Comparative Example.

[0064] Comparative Example 5

[0065] An absorbable biomembrane was prepared as in Example 1, except that the radiation cross-linking dose was 20 kgy, and an absorbable biomembrane of Comparative Example 5 was prepared, which is absorbable biomembrane 5 of Comparative Example.

[0066] Comparative Example 6

[0067] An absorbable biomembrane was prepared as in Example 1, except that the radiation cross-linking dose was 100 kgy, and an absorbable biomembrane of Comparative Example 6 was prepared, which is absorbable biomembrane 6 of Comparative Example.

[0068] The absorbable biofilms obtained in Examples 1-4 and Comparative Examples 1-6 were used for experiments (the experimental method refers to the subcutaneous tissue implantation experimental method in Appendix B of GB / T16886.6-2015) to observe the degradation time of the absorbable biofilm under the skin of New Zealand rabbits. The degradation time of the product was qualified within 6 to 12 weeks. The results are shown in Table 1.

[0069] The absorbable biofilms obtained in Examples 1-4 and Comparative Examples 1-6 were used to conduct an operability test. That is, multiple absorbable biofilms were soaked in saline for more than 1 minute, and one corner was gently grasped with tweezers to take it out of the saline, and transferred to a new container. During this period, the absorbable biofilm was observed to see if it was broken, and the operational breakage rate of each absorbable biofilm was counted. An operational breakage rate greater than 10% was considered unqualified.

[0070] Operational fragmentation rate = number of resorbable biofilms that were fragmented / number of resorbable biofilms that were manipulated × 100%

[0071] The main experimental conditions of all the above embodiments and comparative examples and the in vivo degradation time and operating performance test results of the absorbable biofilms prepared are summarized in Table 1.

[0072] Table 1 Preparation conditions and related indicators of absorbable biofilm

[0073]

[0074]

[0075] From the test results in Table 1, it can be seen that when the HLC protein solution is first kept at 2 to 5°C for more than 2 hours before irradiation cross-linking, a longer degradation time can be achieved with the same or lower protein concentration and / or irradiation dose, and the operating performance of the absorbable biofilm is not significantly affected. After studying this phenomenon, the inventors believe that the reason may be that the HLC can self-assemble to a certain extent at 2 to 5°C to form polymers, and the polymers are fixed due to the subsequent irradiation cross-linking, and even if the temperature returns to room temperature, it does not disaggregate, thereby making the absorbable biofilm difficult to degrade.

[0076] Example 5 Study on the Low-temperature Self-assembly Performance of HLC

[0077] Example 3 of Chinese patent application publication CN115947828A confirms that the HLC does not self-assemble at room temperature. However, further research by the inventors shows that the HLC can self-assemble to a certain extent at low temperatures. Fig. 9 and Fig.10 The transmission electron microscope photos of the collagen solution taken immediately after precooling in Example 1 and Comparative Example 4 show that the HLC self-assembles to a certain extent under the experimental conditions of the examples. Fig. 9 The arrow in the middle points to the protein fibers formed by self-assembly of HLC.

Claims

1. A method for producing an absorbable biofilm, comprising: Step A: precooling a 2-6 wt% collagen aqueous solution to a temperature of 2-5° C. and maintaining the temperature for more than 2 hours; Step B: Immediately placing the pre-cooled collagen aqueous solution at 2-8° C. and irradiating and cross-linking the solution; the irradiation dose for the irradiation and cross-linking is 40-80 kGy; Step C: freeze-drying the irradiated cross-linked collagen aqueous solution to obtain the absorbable biofilm; The amino acid sequence of the collagen is an amino acid sequence obtained by repeating the short amino acid sequence represented by SEQ ID NO: 1 (GAPGAPG SQ GAPG LQ) 52 times.

2. The manufacturing method according to claim 1, wherein: The radiation source for the radiation cross-linking is selected from ultraviolet rays, gamma rays, X-rays, neutron beams, particle beams or electron beams.

3. The manufacturing method according to claim 1, wherein: In the step A, the 2-6 wt % collagen aqueous solution is pre-cooled to a temperature of 2-5° C. and maintained for more than 4 hours.

4. The manufacturing method according to claim 1 further comprises a step D between step A and step B: rapidly freezing the pre-cooled collagen aqueous solution to fix its shape. 5 . The manufacturing method according to claim 1 , further comprising the step of cutting the absorbable biofilm obtained after freeze-drying into a specified size and sterilizing it.

6. The manufacturing method according to claim 1, wherein: The in vivo degradation time of the absorbable biofilm is 6 to 12 weeks.

7. The manufacturing method according to claim 1, wherein: The absorbable biological membrane is an oral collagen membrane.

8. An absorbable biofilm obtained by the production method according to any one of claims 1 to 7.

9. Use of the absorbable biofilm obtained by the manufacturing method according to any one of claims 1 to 7 in the preparation of dental materials, wherein the dental material is an oral collagen membrane, which is used for guided bone regeneration during oral dental implantation, guided bone regeneration around implants during immediate implantation after tooth extraction, guided bone regeneration around implants during delayed implantation after tooth extraction, guided bone regeneration in bone defect areas of bone fracture type, local ridge augmentation, alveolar ridge augmentation, root resection, oral cyst resection and filling of bone defect areas after residual root extraction, and periodontal bone defects.

Citation Information

Cited By

  • Recombinant collagen sponge and manufacturing method thereof

    CN118001452A

  • A recombinant collagen sponge and a method of manufacturing the same

    CN118001452B

  • Preparation method and application of thermo-sensitive collagen-chitosan composite gel

    CN119868635A