Metal film catalytic filter bag and preparation method thereof
By building a foamed nickel-supported catalyst interlayer in the metal film catalytic filter bag, combined with the metal filter bag and porous plate structure, the narrow temperature window and the existing dust and nitrate integrated removal technology of NOX and dust in industrial kiln flue gas are solved. It is susceptible to interference and the equipment occupies a large area, etc., but achieves efficient and low-cost flue gas purification effects.
Patent Information
- Application Number
- CN202410774763.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the integrated removal technology of NOX and dust in industrial kiln flue gas has the following problems: the catalytic filter bag has a narrow temperature window, is susceptible to interference from water and sulfur dioxide, has low catalytic activity, and has limited length and size of the catalytic filter element and is easy to break. Problems such as pipes, large resistance and secondary pollution cause the equipment to occupy a large area and cost high, making it difficult to apply to small and medium-sized kilns.
It adopts a metal film catalytic filter bag with a built-in foam nickel-loaded catalyst interlayer, which is formed by non-woven fabric to provide a high surface area, good thermal conductivity, and porous structure. It combines the metal filter bag and porous plate structure to achieve high-efficiency filtration and catalysis and avoid additional catalyst layers. occupy, improve space utilization and catalyst recycling.
It achieves efficient integrated dust and nitrate removal, reduces system resistance and energy consumption, extends the service life of the catalyst, improves space utilization and recycling, and solves the problems of equipment footprint and high cost in traditional technology.
Smart Images

Figure CN118718588A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of functional filter materials, and mainly to a metal film catalytic filter bag and a preparation method thereof. Background Art
[0002] Industrial combustion produces a large amount of NO X Gases containing sulfuric acid and dust will cause serious environmental problems such as acid rain, photochemical smog, and haze. Unlike the relatively stable and single flue gas operating conditions in the power industry, the non-power industry generally has complex flue gas compositions and is difficult to manage due to its wide range of involvement. Large coal-fired power plants generally adopt the traditional series flue gas purification process in which the denitrification and dust removal units operate independently, which not only occupies a large space, but also has high investment and operating costs. In the past, the removal processes and catalysts for multiple pollutants in large-scale industrial combustion flue gases in the power industry could not be directly applied in the non-power industry. In view of the current status and difficulties of industrial kiln flue gas treatment, the development of advanced materials and technologies that can achieve integrated removal of dust and nitrate is a current research hotspot and important development direction for flue gas purification of small and medium-sized kilns.
[0003] The so-called integrated dust removal technology refers to the use of the same set of technical devices or systems to remove NO in the flue gas in the same smoke temperature range. X And dust are removed at the same time. The core component of the integrated dust and nitrate removal technology is the "catalytic filter" that has both filtering and denitrification functions. According to the different ways of coupling the dust removal filter with the denitrification catalyst and the different substrate carriers, the materials used in the catalytic filter are mainly divided into two categories: catalytic filter bags and catalytic filter elements. The temperature window of the catalytic filter bag is narrow, and it is generally not used in flue gas conditions that are higher than 250°C for a long time. At medium and low temperatures (150-240°C), it is easily interfered by water and sulfur dioxide, which affects the catalytic activity. Catalytic filter elements are more commonly used under medium and high temperature flue gas conditions, but they also have disadvantages such as limited length, easy pipe breakage, large resistance, and secondary pollution. Ordinary metal filter bags require a separate catalyst layer above the filter bag to achieve the function of coordinated governance. For this purpose, a certain amount of floor space and construction costs need to be increased, which hinders the application and promotion of metal filter bags.
[0004] Therefore, it is necessary to develop a catalytic filter material with high precision, high activity, low pressure drop, wide temperature range and high space utilization that is suitable for the needs of industrial kiln flue gas dust removal and denitrification. Summary of the invention
[0005] In view of the problems existing in the prior art, the present application proposes a metal film catalytic filter bag and a preparation method thereof. The present application adopts a metal film as a dust removal filter material, and a built-in catalyst interlayer to realize the dust and saltpeter integrated function. At the same time, the catalyst interlayer is based on a foam nickel formed by a non-woven fabric, and has the characteristics of light weight, high specific surface area, high porosity, strong thermal conductivity and good absorption performance, which can greatly improve the catalytic efficiency and service life of the catalyst.
[0006] According to one aspect of the present application, a metal film catalytic filter bag is proposed, comprising a metal filter bag with a nickel foam loaded catalyst interlayer. The nickel foam has a high surface area and good mass transfer performance, which can effectively improve the utilization rate of the catalyst and reduce the cost; at the same time, the porous structure of the nickel foam is not only conducive to the contact between the catalyst and the reactant, improving the catalytic activity and selectivity, but also can reduce the pressure drop when the fluid passes through the carrier, reducing the energy consumption of the reaction system; and the nickel foam has good high temperature resistance and chemical stability, which can enhance the recyclability and long-term stability of the catalyst in a high temperature environment, and is an excellent carrier for the integral catalyst.
[0007] Furthermore, the nickel foam molding substrate is a non-woven fabric. The non-woven fabric is a material interwoven by fibers or fiber bundles, has a certain pore structure, and can provide the support and template functions required for nickel foam molding. The pore structure of the non-woven fabric is regulated by selecting different fiber densities, weaving methods, or adding pore agents, thereby achieving a customized design of the pore structure of the nickel foam, ensuring the loading effect of the subsequent catalyst active components.
[0008] Furthermore, the nonwoven fabric includes one or more of polyester nonwoven fabric, polyphenylene sulfide nonwoven fabric, polytetrafluoroethylene nonwoven fabric and aramid nonwoven fabric. Polyester nonwoven fabric is a common nonwoven fabric made of synthetic fiber, has low cost and is an ideal base material for forming nickel foam.
[0009] Furthermore, the nickel foam loaded catalyst interlayer is removable and replaceable. The metal filter bag and the built-in catalyst interlayer are relatively independent. After the catalyst performance decreases or becomes inactivated, the catalyst can be separated from the metal filter bag, the catalyst can be regenerated or disposed of separately, and the metal filter bag can be reused. Therefore, compared with catalytic filter bags and catalytic filter elements, metal membrane catalytic filter bags have a higher degree of recycling.
[0010] Furthermore, the metal filter bag is formed by welding the inner layer and the outer layer. This structure enables the foam nickel catalyst interlayer to be firmly fixed in the metal membrane filter bag.
[0011] Specifically, the outer layer is a metal film, and the inner layer is a metal porous plate. The metal film plays a role in filtering dust, while the metal porous plate plays a supporting role without affecting the air permeability and pressure difference of the entire filter bag.
[0012] Specifically, the metal film is a porous filter material of metal compounds made by pressing and sintering metal fibers and metal powders. The metal film can effectively filter dust while protecting the catalyst interlayer, preventing the pores of the nickel foam from being blocked and increasing the service life of the catalyst.
[0013] Specifically, the metal porous plate has evenly distributed holes, a hole diameter of 6-10 mm, and a hole spacing of 9-13 mm. The metal porous plate can cooperate with the metal membrane to fix the foam nickel loaded catalyst interlayer without affecting the passage of flue gas, and can also reduce the problem of catalyst shedding caused by blowing.
[0014] According to the second aspect of the present application, a method for preparing a metal membrane catalytic filter bag is proposed, and the specific steps are as follows:
[0015] S1: preparing nickel foam to form a catalyst carrier;
[0016] S2: loading a catalyst on the nickel foam;
[0017] S3: Assembling the metal membrane catalytic filter bag.
[0018] Furthermore, in S1, the specific preparation method of the nickel foam is as follows: using warm water with added surfactant to wash away grease and impurities on the non-woven fabric; using 5% nitric acid solution to activate the non-woven fabric and wash and dry it; setting the electrodeposition parameters, immersing the non-woven fabric in the electrolyte as a cathode, connecting the anode, applying direct current for electrodeposition, and reducing nickel ions on the surface of the non-woven fabric to form a nickel layer; annealing the non-woven fabric after electrodeposition in a special atmosphere for 1-2 hours to obtain a nickel foam catalyst carrier, and the annealing temperature is 400-600°C. After annealing, the non-woven fabric is burned out to obtain a nickel foam catalyst carrier with light weight, high specific surface area, high porosity, strong thermal conductivity and good absorption performance.
[0019] Specifically, the electrodeposition parameters include a deposition temperature of 25-35°C, a current density of 1-5A / dm 2 The deposition time is 30-60 minutes. Deposition under these conditions can ensure the efficiency and quality of electrodeposition and the performance of the nickel foam deposition layer.
[0020] Specifically, the electrolyte includes 100-200 g / L of nickel sulfate, 40-50 g / L of nickel chloride and 30-60 g / L of boric acid. This electrolyte formula can make the current pass smoothly and promote the smooth progress of the electrodeposition process.
[0021] Specifically, the anode includes stainless steel or titanium metal. Both stainless steel and titanium metal have good electrical conductivity and corrosion resistance and a long service life.
[0022] Specifically, the special atmosphere includes nitrogen or hydrogen, which can fully burn the non-woven fabric without remaining in the nickel foam.
[0023] Furthermore, in S2, the specific loading method of the catalyst is as follows: selecting a catalyst powder catalyst slurry; ball milling the catalyst slurry to a particle size of 1-4 μm; stirring and aging the catalyst slurry for 12-48 hours; loading the catalyst on the nickel foam by coating or impregnation, and drying; calcining and activating the dried sample at a calcination temperature of 300-450°C for 3-6 hours. After calcination, a monolithic catalyst product with firm loading, uniform dispersion, good air permeability, high temperature resistance, certain flexibility and mechanical strength can be obtained.
[0024] Specifically, the catalytic powder is selected from one or more of vanadium-based, manganese-based, iron-based denitration catalysts, denitration molecular sieves and denitration MOFs.
[0025] Specifically, the coating method requires multiple coating and drying, the first coating is dried by microwave, and the remaining coating is dried by hot air. The catalyst loading is 150-1000g / m 2 The coating is stopped when the impregnation method requires multiple impregnation and drying, the first impregnation is dried by microwave, and the remaining impregnation is dried by hot air. The catalyst loading is 150-1000g / m 2 Stop impregnation when the time is short. Microwave drying can quickly combine the catalyst and nickel foam when the first coating or impregnation is used, so as to prevent uneven dispersion of the catalyst slurry and precipitation, and avoid adverse effects on subsequent loading and final catalytic performance. Hot air drying takes a long time, which is more conducive to the electron transfer and chemical bond combination of catalyst molecules during the superposition loading process, while ensuring the porosity and air permeability of the nickel foam loaded catalyst interlayer.
[0026] Compared with the prior art, this application has the following beneficial effects:
[0027] (1) High strength and toughness: Metal film catalytic filter bags can achieve high-efficiency filtration and catalytic effects. Compared with chemical fiber catalytic filter bags, they have the advantages of high mechanical strength, not easy to break, and high temperature resistance; compared with ceramic catalytic filter elements, they have the advantages of strong toughness, not easy to break, and long service life.
[0028] (2) High space utilization: The metal membrane catalytic filter bag has a catalyst interlayer inside the metal filter bag, which avoids the space occupied by the additional catalyst layer. It can make full use of the space of the dust and saltpeter integrated equipment, save equipment space, simplify the equipment structure, and improve the stability and reliability of the system.
[0029] (3) Low air resistance and low energy consumption: Compared with ceramic catalytic filter elements and metal filter bags + external catalyst layers, metal membrane catalytic filter bags have a smaller pressure drop, thereby reducing the resistance of the dust and saltpeter integrated system and reducing energy consumption.
[0030] (4) Recyclable: Since the metal filter bag and the built-in catalyst interlayer in the metal membrane catalytic filter bag are relatively independent, after the catalyst performance declines or becomes inactivated, the catalyst can be separated from the metal filter bag, the catalyst can be regenerated or disposed of separately, and the metal filter bag can be reused. Therefore, compared with catalytic filter bags and catalytic filter elements, metal membrane catalytic filter bags have a higher degree of recycling. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings are included to provide a further understanding of the embodiments and are incorporated into and constitute a part of this specification. The accompanying drawings illustrate the embodiments and are used together with the description to explain the principles of the present invention. It will be easy to recognize other embodiments and many expected advantages of the embodiments because they become better understood by reference to the following detailed description. The elements of the drawings are not necessarily to scale with each other. The same reference numerals refer to corresponding similar parts.
[0032] Figure 1 This is a flow chart for the preparation of the metal membrane catalytic filter bag proposed in this application.
[0033] Figure 2 This is a schematic diagram of the overall structure of the metal membrane catalytic filter bag according to an embodiment of the present application.
[0034] Figure 3 for Figure 2 Cross-sectional view in the direction of BB.
[0035] In the figure, 1-metal film layer, 2-nickel foam catalyst layer, 3-metal porous plate layer. DETAILED DESCRIPTION
[0036] The present application will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It should also be noted that, for ease of description, only the parts related to the relevant invention are shown in the accompanying drawings.
[0037] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0038] Figure 1 The flowchart of the preparation of the metal membrane catalytic filter bag proposed in this application is shown.
[0039] Example 1
[0040] A metal film catalytic filter bag, the specific preparation method of which is as follows:
[0041] S101: Use warm water with added surfactant to wash away grease and impurities on the non-woven fabric; use 5% nitric acid solution to activate the non-woven fabric and wash and dry it; set the electrodeposition parameters, deposition temperature 25-35°C, current density 1-5A / dm 2 and deposition time of 30-60min, immersing the non-woven fabric in an electrolyte including 100-200g / L nickel sulfate, 40-50g / L nickel chloride and 30-60g / L boric acid as a cathode, connecting to an anode, applying direct current for electrodeposition, and reducing nickel ions on the surface of the non-woven fabric to form a nickel layer; annealing the electrodeposited non-woven fabric in a special atmosphere for 1-2h to obtain a foamed nickel catalytic carrier, and the annealing temperature is 400-600°C.
[0042] S102: Select catalyst powder to prepare catalyst slurry; ball-mill the catalyst slurry to a particle size of 1-4 μm; stir and age the catalyst slurry for 12-48 hours; load the catalyst on nickel foam by coating or impregnation, and dry it; calcine and activate the dried sample at a calcination temperature of 300-450°C for 3-6 hours.
[0043] S103: Assemble the metal membrane catalytic filter bag, the overall structure diagram is as follows Figure 2 As shown, Figure 3 Shows Figure 2 Cross-sectional view in the direction of BB.
[0044] The prepared metal membrane catalytic filter bag was tested for denitrification efficiency, pressure difference / air permeability and shedding rate. The test items and test methods are as follows:
[0045] Denitration efficiency test: Cut the sample into discs and put it into the SCR catalyst evaluation device for denitration test. The gas concentration (vol%) is controlled by mass flow meter: NO: 500ppm, NH3: 500ppm, O2: 5%, H2O: 15%, N2 is the balance gas, and the filtration wind speed is 1m / min. The denitration rate calculation formula is η=(C1-C2) / C1×100%, where C1 is the concentration of NOx at the inlet, and C2 is the concentration of NOx at the outlet, which is obtained by flue gas analysis test.
[0046] Pressure difference / air permeability test: Tested according to GB / T 6719-2009.
[0047] Shedding rate test: 3 kg compressed air was used for 10,000 times of spraying. The shedding rate calculation formula is η = (C1-C2) / C3×100%, where C1 is the initial weight of the sample, C2 is the weight after spraying, and C3 is the weight of the loaded active ingredient. The sample was dried at 150°C for 4-6 hours before each weighing.
[0048] Example 2
[0049] A metal film catalytic filter bag, the specific preparation method of which is as follows:
[0050] S201: Use warm water with added surfactant to wash away grease and impurities on the non-woven fabric; use 5% nitric acid solution to activate the non-woven fabric and wash and dry it; set the electrodeposition parameters, deposition temperature 30°C, current density 5A / dm 2 and deposition time of 45 min, immersing the non-woven fabric in an electrolyte including 200 g / L nickel sulfate, 50 g / L nickel chloride and 30 g / L boric acid as a cathode, connecting to an anode, applying direct current for electrodeposition, and nickel ions are reduced on the surface of the non-woven fabric to form a nickel layer; the non-woven fabric after electrodeposition is annealed in a special atmosphere for 2 h to obtain a foamed nickel catalytic carrier, and the annealing temperature is 500°C.
[0051] S202: Use vanadium titanium catalyst to prepare catalyst slurry; ball-mill the catalyst slurry to a particle size of 1-4 μm; stir and age the catalyst slurry for 12 hours; load the catalyst on nickel foam by coating or impregnation, and dry it; calcine and activate the dried sample at a calcination temperature of 420°C and a calcination time of 4 hours.
[0052] S203: Assembling metal membrane catalytic filter bag.
[0053] In this embodiment, the vanadium-titanium catalyst loading is 250 g / m 2 .
[0054] Example 3
[0055] A metal film catalytic filter bag, the specific preparation method of which is consistent with Example 2, the nickel foam is loaded with the same vanadium titanium catalyst, and the catalyst loading is 270g / m 2 .
[0056] Example 4
[0057] A metal film catalytic filter bag, the specific preparation method of which is consistent with Example 2, the nickel foam is loaded with the same vanadium titanium catalyst, and the catalytic loading is 320g / m 2 .
[0058] Example 5
[0059] A metal film catalytic filter bag, the specific preparation method of which is as follows:
[0060] S501: Use warm water with added surfactant to wash away grease and impurities on the non-woven fabric; use 5% nitric acid solution to activate the non-woven fabric and wash and dry it; set the electrodeposition parameters, deposition temperature 30°C, current density 5A / dm 2 and deposition time of 45 min, immersing the non-woven fabric in an electrolyte including 200 g / L nickel sulfate, 50 g / L nickel chloride and 30 g / L boric acid as a cathode, connecting to an anode, applying direct current for electrodeposition, and nickel ions are reduced on the surface of the non-woven fabric to form a nickel layer; the non-woven fabric after electrodeposition is annealed in a special atmosphere for 2 h to obtain a foamed nickel catalytic carrier, and the annealing temperature is 500°C.
[0061] S502: Use ZSM-5 molecular sieve catalyst to prepare catalyst slurry; ball-mill the catalyst slurry to a particle size of 1-4 μm; stir and age the catalyst slurry for 48 hours; load the catalyst on nickel foam by coating or impregnation, and dry it; calcine and activate the dried sample at a calcination temperature of 550°C and a calcination time of 3 hours.
[0062] S503: Assemble the metal membrane catalytic filter bag.
[0063] In this embodiment, the ZSM-5 molecular sieve catalyst loading is 250 g / m 2 .
[0064] Example 6
[0065] A metal film catalytic filter bag, the specific preparation method of which is as follows:
[0066] S601: Use warm water with added surfactant to wash away grease and impurities on the non-woven fabric; use 5% nitric acid solution to activate the non-woven fabric and wash and dry it; set the electrodeposition parameters, deposition temperature 30°C, current density 5A / dm 2 and deposition time of 45 min, immersing the non-woven fabric in an electrolyte including 200 g / L nickel sulfate, 50 g / L nickel chloride and 30 g / L boric acid as a cathode, connecting to an anode, applying direct current for electrodeposition, and nickel ions are reduced on the surface of the non-woven fabric to form a nickel layer; the non-woven fabric after electrodeposition is annealed in a special atmosphere for 2 h to obtain a foamed nickel catalytic carrier, and the annealing temperature is 500°C.
[0067] S602: Use SSZ-13 molecular sieve catalyst to prepare catalyst slurry; ball-mill the catalyst slurry to a particle size of 1-4 μm; stir and age the catalyst slurry for 24 hours; load the catalyst on nickel foam by coating or impregnation, and dry it; calcine and activate the dried sample at a calcination temperature of 550°C for 3 hours.
[0068] S603: Assemble the metal membrane catalytic filter bag.
[0069] In this example, the SSZ-13 molecular sieve catalyst loading is 250 g / m 2 .
[0070] Example 7
[0071] A metal film catalytic filter bag, the specific preparation method of which is as follows:
[0072] S701: Use warm water with added surfactant to wash away grease and impurities on the non-woven fabric; use 5% nitric acid solution to activate the non-woven fabric and wash and dry it; set the electrodeposition parameters, deposition temperature 30°C, current density 5A / dm 2 and deposition time of 45 min, immersing the non-woven fabric in an electrolyte including 200 g / L nickel sulfate, 50 g / L nickel chloride and 30 g / L boric acid as a cathode, connecting to an anode, applying direct current for electrodeposition, and nickel ions are reduced on the surface of the non-woven fabric to form a nickel layer; the non-woven fabric after electrodeposition is annealed in a special atmosphere for 2 h to obtain a foamed nickel catalytic carrier, and the annealing temperature is 500°C.
[0073] S702: Use ZSM-5 & SSZ-13 mixed molecular sieve catalyst to prepare catalyst slurry, wherein the mass ratio of ZSM-5 mixed molecular sieve catalyst to SSZ-13 mixed molecular sieve catalyst is 1:1; ball mill the catalyst slurry particle size to 1-4μm; stir and age the catalyst slurry for 36h; load the catalyst on nickel foam by coating or impregnation method, and dry it; calcine and activate the dried sample at a calcination temperature of 550℃ and a calcination time of 3h.
[0074] S703: Assemble the metal membrane catalytic filter bag.
[0075] In this embodiment, the ZSM-5 & SSZ-13 mixed molecular sieve catalyst loading is 250 g / m 2 .
[0076] Comparative Example 1
[0077] This comparative example is a polytetrafluoroethylene (PTFE) non-woven fabric loaded with a vanadium-titanium catalyst, with a loading of 320 g / m 2 .
[0078] The filter materials of Examples 2-7 and Comparative Example 1 were subjected to performance tests, and the test results are shown in Tables 1-4.
[0079] Table 1 Summary of test results of denitrification efficiency of nickel foam catalyst layer
[0080]
[0081] Table 2 Summary of test results of PTFE catalytic filter material denitrification efficiency
[0082]
[0083] Table 3 Summary of pressure difference test / air permeability test results
[0084]
[0085]
[0086] Table 4 Summary of shedding rate test results
[0087]
[0088] As can be seen from Table 1, the catalytic filter bags formed by using nickel foam as the matrix and loading vanadium-titanium and molecular sieve catalysts have good catalytic performance. Under the conditions of water vapor content of 15% and temperature above 280°C, the denitrification efficiency exceeds 90%, proving that the catalytic filter bags have good water resistance. As can be seen from Table 2, ordinary PTFE catalytic filter bags can only be used under conditions of <240°C, and the denitrification efficiency still does not reach 100% at 240°C, which may be related to the water vapor content. In the temperature gradients of 260°C-340°C and 160°C-240°C, the relationship between the denitrification efficiency and temperature of all catalysts is positively correlated. Compared with vanadium-titanium catalysts, molecular sieves perform better under relatively low temperature conditions. Under the same catalyst loading, the SSZ-13 molecular sieve catalyst performs best, reaching a denitrification efficiency of 100% at 280°C.
[0089] It can be seen from Table 3 that when the resistance is 200Pa, the air permeability of the catalyst layer based on nickel foam is 1000L / dm 2 / min or more, while the air permeability of ordinary PTFE catalytic filter bags is less than 100L / dm 2 / min, which is much lower than the catalytic filter layer based on nickel foam. This proves that the catalytic filter layer based on nickel foam has good air permeability, will not bring resistance burden to the system, and can reduce operating costs.
[0090] It can be seen from Table 4 that the catalyst shedding rate of the overall nickel foam matrix is low, which is better than that of the traditional PTFE filter material even at the same loading amount.
[0091] In summary, the metal membrane catalytic filter bag of the present application has the advantages of high strength, high toughness, high space utilization, high catalytic activity, high catalyst utilization, high catalytic stability, low air permeability and low energy consumption.
[0092] The above describes the specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
[0093] In the description of the present application, it should be understood that the terms "upper", "lower", "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The wording 'comprising' does not exclude the presence of elements or steps not listed in the claims. The wording 'one' or 'an' preceding an element does not exclude the presence of a plurality of such elements. The simple fact that certain measures are recorded in mutually different dependent claims does not indicate that a combination of these measures cannot be used for improvement. Any reference symbols in the claims should not be interpreted as limiting the scope.
Claims
1. A metal film catalytic filter bag, characterized in that: The metal filter bag has a built-in nickel foam loaded catalyst interlayer; the nickel foam forming substrate is a non-woven fabric.
2. The metal film catalytic filter bag according to claim 1, characterized in that: The nickel foam loaded catalyst interlayer is detachable and replaceable.
3. The metal film catalytic filter bag according to claim 1, characterized in that: The non-woven fabric includes one or more of polyester non-woven fabric, polyphenylene sulfide non-woven fabric, polytetrafluoroethylene non-woven fabric and aramid non-woven fabric.
4. The metal film catalytic filter bag according to claim 1, characterized in that: The metal filter bag is formed by welding an inner layer and an outer layer.
5. The metal film catalytic filter bag according to claim 4, characterized in that: The outer layer is a metal film, and the inner layer is a metal porous plate.
6. The metal film catalytic filter bag according to claim 5, characterized in that: The metal film is a porous filtering material of an intermetallic compound made by pressing and sintering metal fibers and metal powders.
7. The metal film catalytic filter bag according to claim 5, characterized in that: The holes of the metal porous plate are evenly distributed, the hole diameter is 6-10mm, and the hole spacing is 9-13mm.
8. A method for preparing a metal film catalytic filter bag, characterized in that: The specific steps are: S1: preparing nickel foam to form a catalyst carrier; S2: loading a catalyst on the nickel foam; S3: Assembling the metal membrane catalytic filter bag.
9. The method for preparing a metal film catalytic filter bag according to claim 8, characterized in that: In S1, the specific preparation method of nickel foam is as follows: use warm water with added surfactant to wash away grease and impurities on the non-woven fabric; use 5% nitric acid solution to activate the non-woven fabric and wash and dry it; set the electrodeposition parameters, immerse the non-woven fabric in the electrolyte as a cathode, connect the anode, apply direct current for electrodeposition, and reduce nickel ions on the surface of the non-woven fabric to form a nickel layer; anneal the non-woven fabric after electrodeposition in a special atmosphere for 1-2 hours to obtain a nickel foam catalytic carrier, and the annealing temperature is 400-600°C.
10. The method for preparing a metal film catalytic filter bag according to claim 9, characterized in that: The electro-deposition parameters include deposition temperature of 25-35°C, current density of 1-5A / dm 2 and deposition time 30-60min.
11. The method for preparing a metal film catalytic filter bag according to claim 9, characterized in that: The electrolyte comprises the following components: 100-200 g / L of nickel sulfate, 40-50 g / L of nickel chloride and 30-60 g / L of boric acid.
12. The method for preparing a metal film catalytic filter bag according to claim 9, characterized in that: The anode includes stainless steel or titanium metal.
13. The method for preparing a metal film catalytic filter bag according to claim 9, characterized in that: The special atmosphere includes nitrogen or hydrogen.
14. The method for preparing a metal film catalytic filter bag according to claim 8, characterized in that: In S2, the specific loading method of the catalyst is as follows: select catalyst powder to prepare catalyst slurry; ball-mill the catalyst slurry to a particle size of 1-4 μm; stir and age the catalyst slurry for 12-48 hours; load the catalyst on nickel foam by coating or impregnation, and dry it; calcine and activate the dried sample at a calcination temperature of 300-450°C and a calcination time of 3-6 hours.
15. The method for preparing a metal film catalytic filter bag according to claim 14, characterized in that: The catalytic powder is selected from one or more of vanadium-based, manganese-based, iron-based denitration catalysts, denitration molecular sieves and denitration MOFs.
16. The method for preparing a metal film catalytic filter bag according to claim 14, characterized in that: The coating method requires multiple coating and drying, the first coating is dried by microwave, and the remaining coating is dried by hot air. The catalyst loading is 150-1000g / m 2 The coating is stopped when the impregnation method requires multiple impregnation and drying, the first impregnation is dried by microwave, and the remaining impregnation is dried by hot air. The catalyst loading is 150-1000g / m 2 Stop dipping.
Citation Information
Patent Citations
Foam iron-nickel composite metal material and preparation method thereof
CN101265549A
Integrated device of bag-type dust removal, catalytic denitration and dioxin removal
CN109126313A
Flue gas desulfurization, denitrification and dust removal integrated device and treatment process thereof
CN113731047A
Metal composite filter cartridge for high-temperature flue gas dust removal and denitration integrated system
CN212757752U