Preparation of coal gangue-based geopolymer microspheres and application of coal gangue-based geopolymer microspheres in adsorption of methylene blue and hexavalent chromium

By preparing geopolymer microspheres with a spherical structure and utilizing their high pore area and modified surface charge, the adsorption effect of methylene blue and hexavalent chromium is significantly improved, solving the problem of pollutant removal in printing and dyeing wastewater, and achieving economical and efficient utilization of waste resources.

CN118718995AActive Publication Date: 2024-10-01FUZHOU UNIV

Patent Information

Application Number
CN202410765347.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively remove methylene blue and hexavalent chromium from printing and dyeing wastewater, leading to environmental pollution and health risks, and the adsorbent is costly and difficult to regenerate.

Method used

Geopolymer microspheres with a spherical structure are prepared by mixing gangue, fly ash, slag, alkali activators, foaming agents and composite modifiers, and use their high pore area and modified surface charge to significantly improve methylene blue and hexavalent chromium adsorption effect.

Benefits of technology

It achieves efficient adsorption of methylene blue and hexavalent chromium, reduces adsorbent preparation costs, solves the problems of industrial solid waste accumulation and environmental pollution, and provides conditions for high-value utilization of industrial solid waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718995A_ABST
    Figure CN118718995A_ABST
Patent Text Reader

Abstract

The invention discloses preparation of coal gangue-based geopolymer microspheres and application of the coal gangue-based geopolymer microspheres to adsorption of methylene blue and hexavalent chromium, and the geopolymer microspheres are prepared by mixing coal gangue, fly ash, slag, an alkali activator, a foaming agent and a composite modifier. The geopolymer with a spherical structure is successfully prepared through the three solid powder materials, the prepared geopolymer has a large pore area and a large number of pits and gullies on the surface through the synergistic effect of the three solid powder materials, and more adsorption active sites can be provided; the composite modifier is added, so that the adsorption effect of methylene blue and hexavalent chromium can be remarkably improved, and secondary utilization of waste resources is realized; the problems of accumulation of industrial solid wastes such as coal gangue and environmental pollution are effectively solved, favorable conditions are provided for high-value utilization of the industrial solid wastes, and the method has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a geopolymer and a preparation method and application thereof, and in particular to the preparation of coal gangue-based geopolymer microspheres and the application thereof in adsorbing methylene blue and hexavalent chromium. Background Art

[0002] Methylene blue is one of the common organic pollutants in printing and dyeing wastewater. It is widely used in dyeing hemp, silk fabrics, paper, bamboo and wood, and can also be used to make inks and lakes and dye biological and bacterial tissues. However, methylene blue wastewater has the characteristics of high chroma and difficulty in degradation. Discharging into rivers will cause serious discoloration of river water, destroy the transparency of water bodies, and affect the survival of aquatic organisms. In addition, methylene blue and its metabolites are also teratogenic, and long-term exposure may pose a potential threat to human health. On the other hand, hexavalent chromium is another important inorganic pollutant in printing and dyeing wastewater. Chromium exists in various valence states in nature, among which hexavalent chromium is the most toxic. Hexavalent chromium compounds are highly oxidizing and toxic, and can invade the human body through various pathways, such as the digestive tract, respiratory tract, skin and mucous membranes. Long-term contact or ingestion of hexavalent chromium may cause a variety of health problems, such as skin damage, respiratory diseases, digestive system diseases and even cancer.

[0003] In view of these problems, it is urgent to study other effective methods to reduce the adverse effects of methylene blue and hexavalent chromium in printing and dyeing wastewater on the environment. It is extremely important to develop economically feasible technologies to remove methylene blue and hexavalent chromium from the environment. The methods for treating printing and dyeing wastewater include three categories: physical, chemical and biological. Physical methods such as adsorption and membrane separation remove suspended matter and dyes in wastewater through physical action. Chemical methods such as coagulation and oxidation use chemical reactions to change the properties of wastewater, reduce color and remove pollutants. Biological methods use the degradation of microorganisms to remove organic matter from wastewater. Because adsorption is simple and environmentally friendly, adsorption has become a better way to treat methylene blue and hexavalent chromium.

[0004] Studies have shown that adsorbent cost and regeneration are the main factors limiting the development of adsorption methods, and it is urgent to develop economical, efficient and renewable adsorbents. Geopolymers, as a new type of gelling material, have attracted more and more researchers' attention due to their potential as adsorbents. Summary of the invention

[0005] The purpose of the present invention is to solve the above-mentioned technical problems. The invention discloses the preparation of coal gangue-based geopolymer microspheres and their application in adsorbing methylene blue and hexavalent chromium. The geopolymer microspheres are prepared by mixing coal gangue, fly ash, slag, alkali activator, foaming agent and composite modifier. By modifying and utilizing industrial waste coal gangue, fly ash and slag, geopolymers with spherical structures are successfully prepared. The prepared geopolymer has a higher pore area through the synergistic effect between the three solid powders, and has a large number of depressions and gullies on the surface, which can provide more adsorption active sites; adding the composite modifier can significantly improve the adsorption effect of methylene blue and hexavalent chromium, while removing methylene blue from water, it can also improve the removal effect of hexavalent chromium, reduce the preparation cost of the adsorbent and realize the resource utilization of solid waste; effectively solve the problems of accumulation and environmental pollution of industrial solid wastes such as coal gangue, provide favorable conditions for the high-value utilization of industrial solid wastes, and have good application prospects.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] Gangue-based polymer microspheres, including the following raw materials:

[0008] Solid powder: coal gangue, fly ash, slag; wherein the mass fraction of coal gangue in the solid powder is 25-50%; the mass fraction of fly ash is 25-50%; the mass fraction of slag is 25-50%; the sum of the mass fractions of the three is 100%;

[0009] Alkali activator: water glass and sodium hydroxide, wherein the mass ratio of water glass to sodium hydroxide is 53-112:10; the mass ratio of water glass to solid powder is 3-5:10;

[0010] Foaming agent: hydrogen peroxide solution, the mass ratio of the hydrogen peroxide solution to the solid powder is 0.6-0.8:100;

[0011] Modifier: dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline, the mass ratio of dodecyltrimethylammonium bromide DTAB to solid powder is 1-30:100; the mass ratio of 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline to solid powder is 1-30:100.

[0012] Furthermore, the mass percentage of each component in the coal gangue is: SiO2: 60%-70%, Al2O3: 20%-30%, CaO: 0.1%-1%, K2O: 3%-4%, TiO2: 1%-2%; the mass percentage of each component in the fly ash is: SiO2: 50%-60%, Al2O3: 35%-45%, CaO: 0.01%-0.1%, K2O: 1%-2%, TiO2: 2%-3%; the mass percentage of each component in the slag is: SiO2: 30%-40%, Al2O3: 10%-20%, CaO: 30%-40%, K2O: 0.1%-1%, TiO2: 1%-2%.

[0013] Furthermore, the particle size of the coal gangue is less than 0.075 mm, and it needs to be calcined at 600-800° C. for 4-6 hours before use; the particle size of the fly ash is less than 0.075 mm, and the particle size of the slag is less than 0.075 mm.

[0014] Furthermore, the modulus of the water glass is 1.2-1.8, the solid content is 34wt%, and the Baume degree is 40; and the concentration of the hydrogen peroxide solution is 10wt%-30wt%.

[0015] The preparation method of coal gangue-based polymer microspheres comprises the following steps:

[0016] Step S1: uniformly mixing coal gangue, fly ash, slag, dodecyltrimethylammonium bromide (DTAB) and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline in proportion to obtain a solid mixture A;

[0017] Step S2: mixing water glass and sodium hydroxide in proportion, stirring and mixing, and then standing to obtain an alkali activator;

[0018] Step S3: The hydrogen peroxide solution is taken out and sealed for later use to obtain a foaming agent;

[0019] Step S4: adding the solid mixture A obtained in step S1 to the alkali activator obtained in step S2; after mixing, mechanically stirring to obtain a mixed slurry B;

[0020] Step S5: adding the foaming agent obtained in step S3 to the mixed slurry B obtained in step S4, and then mechanically stirring to obtain a mixed slurry C;

[0021] Step S6: vertically drop the mixed slurry C into a dimethyl silicone oil bath for dispersion and molding;

[0022] Step S7: collecting the formed microspheres by suction filtration and placing them in a blast drying oven for curing and solidification;

[0023] Step S8: placing the cured microspheres in a muffle furnace and calcining to remove excess dimethyl silicone oil.

[0024] Furthermore, the alkaline activator is allowed to stand for 12-24 hours, the dimethyl silicone oil bath temperature is 70-85°C, the dispersion molding time is 10-20 minutes, the blast drying oven curing temperature is 60-80°C, the curing time is 0.5-1.0 hours, the calcination temperature is 250-350°C, and the calcination time is 2-3 hours.

[0025] The application method of gangue-based polymer microspheres in adsorbing methylene blue and hexavalent chromium comprises: mixing and stirring the gangue-based polymer microspheres with wastewater;

[0026] The wastewater is wastewater containing methylene blue solution and / or hexavalent chromium solution.

[0027] Furthermore, the stirring time is 100-120 min.

[0028] Furthermore, the concentration of methylene blue and / or hexavalent chromium in the wastewater is 10-200 mg / L, the pH value is 1.5-10, and the peak value of the ultraviolet spectrum is 500-700 nm.

[0029] Furthermore, the dosage of the gangue-based polymer microspheres is 1.0-10 g / L, and the stirring rate is 800-1000 r / min.

[0030] The beneficial effects of the present invention are:

[0031] (1) Geopolymer microspheres with spherical structures were successfully prepared by modifying and utilizing industrial wastes such as coal gangue, fly ash and slag, and were used for the adsorption of methylene blue and hexavalent chromium;

[0032] (2) The solid powders and composite modifier components of the present invention are used to play a synergistic role. The prepared geopolymer has a higher pore area, can provide more adsorption sites, and can change the surface charge of the geopolymer, so that the geopolymer microspheres significantly improve the adsorption effect of methylene blue and hexavalent chromium;

[0033] (3) It uses a wide range of raw material sources, implements green and environmentally friendly preparation processes, has no CO2 emissions, reduces production costs, effectively solves the problems of industrial solid waste accumulation and environmental pollution, and provides favorable conditions for the high added value utilization of industrial solid waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a SEM full picture of the geopolymer microspheres prepared in Example 1 of the present invention;

[0035] Figure 2This is a surface image of the geopolymer microspheres prepared in Example 1 of the present invention;

[0036] Figure 3 This is a surface image of the geopolymer microspheres prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The following will further describe the optimized implementation of the present invention. Although the following describes the optimized implementation of the present invention, it should be understood that the present invention can be implemented in various forms and should not be limited by the implementation described here. On the contrary, these implementations are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art. At the same time, the protection scope of the present invention includes but is not limited to the following:

[0038] The mass percentages of the raw materials used in the geopolymer microspheres in the following embodiments are: coal gangue: fly ash: slag are 25-50%: 25-50%: 25-50%. Water glass is a commercially available chemical agent with a modulus of 1.2-1.8, a solid content of 34wt%, a Baume degree of 40, and the amount of water glass added is 30wt%-50wt% of the solid powder, and the amount of sodium hydroxide added is 3.57wt%-7.5wt% of the solid powder. The purity of the hydrogen peroxide used is analytically pure, with a percentage of 30%, and the amount added is 0.6wt%-0.8wt% of the solid powder. The DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline used are commercially available chemical agents, chemically pure, and the amount added is 30wt% of the solid powder. The dimethyl silicone oil bath temperature is 85°C, the dispersion molding time is 15 minutes, the blast drying oven curing temperature is 80°C, the curing time is 1.0 hour, the calcination temperature is 300°C, and the calcination time is 2 hours.

[0039] The water used in the following examples is tap water.

[0040] The concentrations of the wastewater (methylene blue and hexavalent chromium) in the embodiment of the present invention are determined by the absorption peak intensities of an ultraviolet spectrophotometer at 664 nm and 544 nm, respectively.

[0041] Example 1

[0042] The geopolymer microspheres of this embodiment include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fractions of coal gangue and fly ash in the solid powder are 25% (25g) and 25% (25g) respectively, and the mass fraction of slag is 50% (50g); the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g) respectively in the solid powder; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution as the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0043] After coal gangue, fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0044] Take 50mL, 100mg / L, 25℃ wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500mg of geopolymer microspheres and add them to the solution, stir for 120min, and detect with a UV spectrophotometer.

[0045] Example 2

[0046] The geopolymer microspheres of this embodiment include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fractions of coal gangue and fly ash in the solid powder are 30% (30g) and 30% (30g) respectively, and the mass fraction of slag is 40% (40g); the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 20% (20g) and 10% (10g) of the solid powder respectively; the modulus of water glass in the alkali activator is 1.2, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 7.5wt% (7.5g) of the solid powder; the addition amount of hydrogen peroxide solution as the foaming agent is 0.6wt% (0.6g) of the solid powder.

[0047] After coal gangue, fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0048] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0049] Example 3

[0050] The geopolymer microspheres of this embodiment include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fractions of coal gangue and fly ash in the solid powder are 35% (35g) and 35% (35g) respectively, and the mass fraction of slag is 30% (30g); the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g) respectively; the modulus of water glass in the alkali activator is 1.2, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 7.5wt% (7.5g) of the solid powder; the addition amount of hydrogen peroxide solution as the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0051] After coal gangue, fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0052] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0053] Example 4

[0054] The geopolymer microspheres of this embodiment include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fractions of coal gangue and fly ash in the solid powder are 50% (50g) and 25% (25g) respectively, and the mass fraction of slag is 25% (25g); the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 10% (10g) and 20% (20g) of the solid powder respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution as the foaming agent is 0.6wt% (0.6g) of the solid powder.

[0055] After coal gangue, fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0056] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0057] Example 5

[0058] The geopolymer microspheres of this embodiment include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fractions of coal gangue and fly ash in the solid powder are 25% (25g) and 50% (50g) respectively, and the mass fraction of slag is 25% (25g); the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 20% (20g) and 10% (10g) of the solid powder respectively; the modulus of water glass in the alkali activator is 1.8, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 3.57wt% (3.57g) of the solid powder; the addition amount of hydrogen peroxide solution as the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0059] After coal gangue, fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0060] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0061] Example 6

[0062] The geopolymer microspheres of this embodiment include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fractions of coal gangue and fly ash in the solid powder are 40% (40g) and 30% (30g) respectively, and the mass fraction of slag is 30% (30g); the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g) respectively; the modulus of water glass in the alkali activator is 1.8, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 3.57wt% (3.57g) of the solid powder; the addition amount of hydrogen peroxide solution as the foaming agent is 0.6wt% (0.6g) of the solid powder.

[0063] After coal gangue, fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0064] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0065] Example 7

[0066] The geopolymer microspheres of this embodiment include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fractions of coal gangue and fly ash in the solid powder are 30% (30g) and 35% (35g) respectively, and the mass fraction of slag is 35% (35g); the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 10% (10g) and 20% (20g) of the solid powder respectively; the modulus of water glass in the alkali activator is 1.2, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 7.5wt% (7.5g) of the solid powder; the addition amount of hydrogen peroxide solution as the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0067] After coal gangue, fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0068] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0069] The degradation effect of the wastewater (methylene blue or hexavalent chromium) of Examples 1-7 was tested, and the results are shown in Table 1.

[0070] Table 1 Degradation effect of wastewater (methylene blue or hexavalent chromium) in the embodiment

[0071]

[0072]

[0073] With reference to Example 1, the following comparative examples are set:

[0074] Comparative Example 1

[0075] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 0 (0g), the mass fractions of fly ash and slag are 50% (50g) and 50% (50g) respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g) respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0076] After fly ash, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0077] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0078] Comparative Example 2

[0079] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 50% (50g), and the mass fractions of fly ash and slag are 0 (0g) and 50% (50g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g), respectively; the modulus of water glass in the alkali activator is 1.4, and the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0080] After coal gangue, slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0081] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0082] Comparative Example 3

[0083] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 50% (50g), the mass fractions of fly ash and slag are 50% (50g) and 0 (0g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g), respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0084] After coal gangue, fly ash, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0085] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0086] Comparative Example 4

[0087] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 25% (25g), the mass fractions of fly ash and slag are 25% (25g) and 50% (50g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 30% (30g) and 0 (0g), respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0088] After uniformly mixing coal gangue, fly ash, slag and dodecyltrimethylammonium bromide DTAB in the above proportions, add water glass, sodium hydroxide and foaming agent in proportion, stir mechanically and evenly pour into a syringe, vertically drop into a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes, collect the molded microspheres by suction filtration, put them into a forced air drying oven at 80°C for curing and curing for 1.0 hour, and then calcine at 300°C in a muffle furnace for 2 hours.

[0089] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0090] Comparative Example 5

[0091] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 25% (25g), the mass fractions of fly ash and slag are 25% (25g) and 50% (50g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 0 (0g) and 30% (30g), respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0092] After coal gangue, fly ash, slag and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, and vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes. The molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0093] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0094] Comparative Example 6

[0095] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 100% (100g), the mass fractions of fly ash and slag are 0 (0g) and 0 (0g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g), respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0096] After coal gangue, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0097] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0098] Comparative Example 7

[0099] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 0 (0g), and the mass fractions of fly ash and slag are 100% (100g) and 0 (0g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g), respectively; the modulus of water glass in the alkali activator is 1.4, and the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0100] After fly ash, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a forced air drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0101] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0102] Comparative Example 8

[0103] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 0 (0g), and the mass fractions of fly ash and slag are 0 (0g) and 100% (100g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 15% (15g) and 15% (15g), respectively; the modulus of water glass in the alkali activator is 1.4, and the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0104] After mixing slag, dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline in the above proportions, add water glass, sodium hydroxide and foaming agent in proportion, stir mechanically and pour into a syringe, vertically drop into a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes, collect the molded microspheres by suction filtration, put them into a forced air drying oven at 80°C for curing and curing for 1.0 hour, and then calcine at 300°C in a muffle furnace for 2 hours.

[0105] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0106] Comparative Example 9

[0107] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 0 (0g), and the mass fractions of fly ash and slag are 50% (50g) and 50% (50g) respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 30% (30g) and 0 (0g) respectively; the modulus of water glass in the alkali activator is 1.4, and the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0108] After fly ash, slag and dodecyltrimethylammonium bromide DTAB are evenly mixed in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, and vertically dropped in a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes. The molded microspheres are collected by filtration, placed in a forced air drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0109] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0110] Comparative Example 10

[0111] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 50% (50g), and the mass fractions of fly ash and slag are 0 (0g) and 50% (50g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 30% (30g) and 0 (0g), respectively; the modulus of water glass in the alkali activator is 1.4, and the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0112] After the gangue, slag and dodecyltrimethylammonium bromide DTAB are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, the mixture is evenly poured into a syringe after mechanical stirring, and vertically dropped into a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes. The molded microspheres are collected by filtration, placed in a forced air drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0113] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0114] Comparative Example 11

[0115] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 50% (50g), the mass fractions of fly ash and slag are 50% (50g) and 0 (0g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 30% (30g) and 0 (0g), respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0116] After coal gangue, fly ash and dodecyltrimethylammonium bromide DTAB are evenly mixed in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, and vertically dropped in a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes. The molded microspheres are collected by filtration, placed in a forced air drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0117] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0118] Comparative Example 12

[0119] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 0 (0g), and the mass fractions of fly ash and slag are 50% (50g) and 50% (50g) respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 0 (0g) and 30% (30g) respectively; the modulus of water glass in the alkali activator is 1.4, and the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0120] After fly ash, slag and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline are uniformly mixed in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes, the molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0121] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0122] Comparative Example 13

[0123] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 50% (50g), and the mass fractions of fly ash and slag are 0 (0g) and 50% (50g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 0 (0g) and 30% (30g), respectively; the modulus of water glass in the alkali activator is 1.4, and the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0124] After coal gangue, slag and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline are mixed evenly in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, and vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes. The molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0125] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0126] Comparative Example 14

[0127] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 50% (50g), the mass fractions of fly ash and slag are 50% (50g) and 0 (0g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 0 (0g) and 30% (30g), respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0128] After coal gangue, fly ash and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline are uniformly mixed in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, and vertically dropped in a 85°C dimethyl silicone oil bath for dispersion and molding for 15 minutes. The molded microspheres are collected by suction filtration, placed in a blast drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0129] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0130] Comparative Example 15

[0131] The geopolymer microspheres of this comparative example include coal gangue, fly ash, slag, alkali activator, foaming agent and modifier. The mass fraction of coal gangue in the solid powder is 100% (100g), the mass fractions of fly ash and slag are 0 (0g) and 0 (0g), respectively; the mass fractions of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline in the modifier are 30% (30g) and 0 (0g), respectively; the modulus of water glass in the alkali activator is 1.4, the addition amount is 40wt% (40g) of the solid powder, and the addition amount of sodium hydroxide is 5.81wt% (5.81g) of the solid powder; the addition amount of hydrogen peroxide solution in the foaming agent is 0.8wt% (0.8g) of the solid powder.

[0132] After coal gangue and dodecyltrimethylammonium bromide DTAB are evenly mixed in the above proportions, water glass, sodium hydroxide and foaming agent are added in proportion, mechanically stirred evenly, poured into a syringe, and vertically dropped in a dimethyl silicone oil bath at 85°C for dispersion and molding for 15 minutes. The molded microspheres are collected by filtration, placed in a forced air drying oven at 80°C for curing and curing for 1.0 hour, and then calcined at 300°C in a muffle furnace for 2 hours.

[0133] Take 50 ml, 100 mg / L, 25°C wastewater (methylene blue or hexavalent chromium) solution as the target pollutant, weigh 500 mg of geopolymer microspheres and add them to the solution, stir for 120 min, and detect using a UV spectrophotometer.

[0134] The adsorption effect of the organic matter (methylene blue or hexavalent chromium) in Comparative Examples 1-15 was tested, and the results are shown in Table 2.

[0135] Table 2 Degradation effect of comparative wastewater (methylene blue or hexavalent chromium)

[0136]

[0137]

[0138]

[0139] like Figure 1 and Figure 2 As shown in Table 1, it can be seen that the geopolymer microspheres have obvious adsorption effects on methylene blue and hexavalent chromium, especially in Example 1, the removal rate of methylene blue reaches 94.72%, which is due to the excellent pore structure of the geopolymer prepared by the synergistic use of the three solid powders and the rich hydroxyl structure on the surface of the geopolymer microspheres, which can adsorb methylene blue through pores and electrostatic adsorption. At the same time, the rich hydroxyl groups on the surface of the geopolymer can react with the nitrogen element in the methylene blue to form a hydrogen bond structure. At the same time, it can be seen from Table 1 that the maximum removal rate of hexavalent chromium by geopolymer microspheres to which DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline modifiers are added is 95.66%. This is because the geopolymer surface is positively charged by the composite modification of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline, which is beneficial to the adsorption of hexavalent chromium in the form of anions in aqueous solution. The composite synergistic modification of DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline makes the maximum removal rate of hexavalent chromium by geopolymer microspheres reach more than 95%, and the effect is extremely significant. Therefore, according to the components of the present invention, geopolymer microspheres with higher pore area and excellent adsorption effect of anionic and cationic pollutants can be obtained.

[0140] like Figure 3 As shown in Table 2, it can be seen that as long as any one or more components of the present invention are missing, the effect of adsorbing methylene blue and hexavalent chromium is significantly reduced. The main reason is that without any one or more components in the solid powder of the present invention, it is impossible to obtain an excellent pore structure geopolymer, so that its ability to expose active sites is not outstanding, the charge modification site is also sharply reduced, and it is impossible to better synergistically change the surface charge of the geopolymer microspheres, resulting in a significant decrease in the adsorption effect of methylene blue and hexavalent chromium.

[0141] In summary, the present invention discloses the preparation of coal gangue-based polymer microspheres and their application in adsorbing methylene blue and hexavalent chromium. The geopolymer microspheres are prepared by mixing coal gangue, fly ash, slag, alkali activator, foaming agent and composite modifier. By modifying and utilizing industrial waste coal gangue, fly ash and slag, geopolymers with spherical structures are successfully prepared. The prepared geopolymer has a higher pore area through the synergistic effect between the three solid powders, and has a large number of depressions and gullies on the surface, which can provide more adsorption active sites; adding the composite modifier can significantly improve the adsorption effect of methylene blue and hexavalent chromium, and realize the secondary utilization of waste resources; it effectively solves the problems of accumulation and environmental pollution of industrial solid wastes such as coal gangue, provides favorable conditions for high-value utilization of industrial solid wastes, and has good application prospects.

[0142] Thus far, various embodiments of the present invention have been described, and the above description is exemplary, not exhaustive, and is not limited to the described embodiments. Without departing from the scope and spirit of the described embodiments, many modifications and variations are within the scope of the present invention for those of ordinary skill in the art.

Claims

1. A coal gangue-based polymer microsphere, characterized in that: Including the following ingredients: Solid powder: coal gangue, fly ash, slag; wherein the mass fraction of coal gangue in the solid powder is 25-50%; the mass fraction of fly ash is 25-50%; the mass fraction of slag is 25-50%; the sum of the mass fractions of the three is 100%; Alkali activator: water glass and sodium hydroxide, wherein the mass ratio of water glass to sodium hydroxide is 53-112:10; the mass ratio of water glass to solid powder is 3-5:10; Foaming agent: hydrogen peroxide solution, the mass ratio of the hydrogen peroxide solution to the solid powder is 0.6-0.8:100; Modifier: dodecyltrimethylammonium bromide DTAB and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline, the mass ratio of dodecyltrimethylammonium bromide DTAB to solid powder is 1-30:100; the mass ratio of 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline to solid powder is 1-30:

100.

2. The gangue-based polymer microspheres according to claim 1, characterized in that: The mass percentage of each component in the coal gangue is: SiO2: 60%-70%, Al2O3: 20%-30%, CaO: 0.1%-1%, K2O: 3%-4%, TiO2: 1%-2%; the mass percentage of each component in the fly ash is: SiO2: 50%-60%, Al2O3: 35%-45%, CaO: 0.01%-0.1%, K2O: 1%-2%, TiO2: 2%-3%; the mass percentage of each component in the slag is: SiO2: 30%-40%, Al2O3: 10%-20%, CaO: 30%-40%, K2O: 0.1%-1%, TiO2: 1%-2%.

3. The gangue-based polymer microspheres according to claim 1, characterized in that: The particle size of the coal gangue is less than 0.075 mm and needs to be calcined at 600-800°C for 4-6 hours before use; the particle size of the fly ash is less than 0.075 mm and the particle size of the slag is less than 0.075 mm.

4. The gangue-based polymer microspheres according to claim 1, characterized in that: The modulus of the water glass is 1.2-1.8, the solid content is 34wt%, and the Baume degree is 40; the concentration of the hydrogen peroxide solution is 10wt%-30wt%.

5. The method for preparing gangue-based polymer microspheres according to claim 1, characterized in that: The steps include: Step S1: uniformly mixing coal gangue, fly ash, slag, dodecyltrimethylammonium bromide (DTAB) and 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline in proportion to obtain a solid mixture A; Step S2: mixing water glass and sodium hydroxide in proportion, stirring and mixing, and then standing to obtain an alkali activator; Step S3: The hydrogen peroxide solution is taken out and sealed for later use to obtain a foaming agent; Step S4: adding the solid mixture A obtained in step S1 to the alkali activator obtained in step S2; after mixing, mechanically stirring to obtain a mixed slurry B; Step S5: adding the foaming agent obtained in step S3 to the mixed slurry B obtained in step S4, and then mechanically stirring to obtain a mixed slurry C; Step S6: vertically drop the mixed slurry C into a dimethyl silicone oil bath for dispersion and molding; Step S7: collecting the formed microspheres by suction filtration and placing them in a blast drying oven for curing and solidification; Step S8: placing the cured microspheres in a muffle furnace and calcining to remove excess dimethyl silicone oil.

6. The method for preparing gangue-based polymer microspheres according to claim 5, characterized in that: The dimethyl silicone oil bath temperature is 70-85 ℃, the dispersion molding time is 10-20 min, the blast drying oven curing temperature is 60-80 ℃, the curing time is 0.5-1.0 h, the calcination temperature is 250-350 ℃, and the calcination time is 2-3 h.

7. Use of the gangue-based polymer microspheres according to any one of claims 1 to 4 in the adsorption of methylene blue and hexavalent chromium, characterized in that: The gangue-based polymer microspheres are mixed and stirred with wastewater; the wastewater is wastewater containing methylene blue solution and / or hexavalent chromium solution.

8. The use according to claim 7, characterized in that The stirring time is 100-120 min.

9. The use according to claim 7, characterized in that The concentration of methylene blue and / or hexavalent chromium in the wastewater is 10-200 mg / L, the pH value is 1.5-10, and the peak value of the ultraviolet spectrum is 500-700 nm.

10. The use according to claim 7, characterized in that The dosage of the gangue-based polymer microspheres is 1.0-10 g / L, and the stirring rate is 800-1000 r / min.

Citation Information

Patent Citations

  • Preparation method and application of hexavalent chromium contaminated soil conditioner

    CN105694894A

  • Solidification / stabilization material and solidification method for lead and chrome in trash incineration fly ash

    CN109647859A

  • Red mud-based sewage treatment agent and preparation method thereof, red mud-based ceramsite concrete and preparation method thereof, and applications

    US20220143571A1

Cited By

  • Preparation method and application of electrolytic manganese slag-fire coal slag-based geopolymer microsphere adsorption material

    CN121134894A