Adsorbent for blood purification and preparation method thereof

By coupling imino diethyl sulfonic acid, hydroxyl, and carboxyl polymer ligands on the surface of polymer microspheres, the efficient removal of low-density lipoproteins and very low-density lipoproteins in the blood is achieved, solving the problems faced by existing technologies. The problem of insufficient selectivity of adsorbents in the medium is eliminated, and the blood purification effect is significantly improved.

CN118719015APending Publication Date: 2024-10-01SUZHOU PUZHAO MEDICAL TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410812525.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When existing blood purification adsorbents remove low-density lipoproteins and very-low-density lipoproteins from the blood, it is difficult to maintain selectivity for beneficial components, and their adsorption effects are limited.

Method used

It uses chain polymers coupled with imino diethyl sulfonic acid, hydroxyl groups, and carboxyl groups as ligands and is fixed on the surface of polymer microspheres to effectively remove low-density lipoproteins and very low-density lipoproteins through electrostatic attraction. At the same time, it reduces the adsorption of high-density lipoprotein.

Benefits of technology

It achieves the removal of more than 70% of low-density lipoproteins and more than 60% of very low-density lipoproteins in the blood, and the non-specific adsorption rate of high-density lipoproteins is less than 20%, significantly improving the selectivity and effect of the adsorbent. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004906525130000021
    Figure BDA0004906525130000021
  • Figure BDA0004906525130000031
    Figure BDA0004906525130000031
  • Figure BDA0004906525130000051
    Figure BDA0004906525130000051
Patent Text Reader

Abstract

The invention relates to an adsorbent for blood purification and a preparation method of the adsorbent. The adsorbent comprises polymer microspheres serving as a carrier and ligands immobilized on the surface of the carrier, the ligand is a chain polymer coupled with iminodiethanesulfonic acid, hydroxyl and carboxyl. The surface of the prepared adsorbent is provided with a large number of negative charges, so that the adsorbent can act with LDL and VLDL with positive charges on the surfaces to generate an adsorption effect, meanwhile, the adsorbent has no obvious adsorption effect on beneficial components such as high-density lipoprotein in blood, and the loss of beneficial protein is less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical polymer materials, and in particular relates to an adsorbent with a new polymer ligand for blood purification and a preparation method thereof. Background Art

[0002] Blood purification is a blood purification technology that directly draws blood out of the body and uses adsorbents to remove harmful substances in the blood. It has excellent clinical reference value for cardiovascular diseases such as atherosclerosis and is currently a technology that is widely used in clinical practice. The components of human blood are complex, among which excessive levels of low-density lipoprotein (LDL), very low-density lipoprotein (VLDL), total cholesterol (TC), triglycerides (TG), etc. are the main factors that cause atherosclerosis and hyperlipidemia pancreatitis, and are components that need to be removed by blood purification. However, other similar components in the blood, such as high-density lipoprotein, are beneficial lipoproteins, and adsorbents are required to retain beneficial substances as much as possible while removing harmful substances, which places high demands on the selectivity of the adsorbent.

[0003] CN109092261A proposes an adsorption scavenger for removing low-density lipoprotein in the blood and a preparation method thereof, comprising polysaccharide microspheres as carriers, and polysaccharide ligands immobilized on the surface of the carriers, wherein the polysaccharide ligands are coupled with hydrophobic chains and anionic groups, and the selective adsorption effect of the ligands on LDL is jointly improved from three aspects: selective adsorption of cyclodextrin and LDL, affinity adsorption of hydrophobic chains and lipids, and electrostatic adsorption of anionic groups and LDL.

[0004] CN109092262 B discloses a low-density lipoprotein adsorption microsphere, on which heparin and delta-tocopherol or alpha-tocopherol capable of adsorbing to the hydrophobic region of LDL are coupled as hydrophobic functional groups, thereby significantly improving the adsorption selectivity for LDL.

[0005] Heparin is a substance with sulfonic acid, hydroxyl and carboxyl groups. CN118002097A and CN104525155A both use heparin as a ligand combined with a resin carrier to prepare an adsorbent for the adsorption of lipoprotein in the blood.

[0006] How to develop adsorbents with broader adsorption effects and better selectivity has become an urgent problem to be solved. Summary of the invention

[0007] The purpose of the present invention is to provide a new adsorbent for blood purification with excellent selectivity, which can selectively remove low-density lipoprotein and very low-density lipoprotein in the blood, but has no obvious adsorption effect on beneficial components in the blood such as high-density lipoprotein, and its preparation method.

[0008] The solution adopted by the present invention to solve the above technical problems is:

[0009] An adsorbent for removing low-density lipoprotein in blood comprises polymer microspheres as carriers and ligands immobilized on the surface of the carriers; the ligands are chain polymers coupled with iminodiethanesulfonic acid, hydroxyl groups and carboxyl groups.

[0010] Furthermore, the polymer microspheres are selected from one of cellulose microspheres, agarose microspheres, dextran microspheres, polyvinyl alcohol microspheres, polyacrylate microspheres, polystyrene microspheres, and polyacrylic acid microspheres.

[0011] Furthermore, the ligand is a copolymer, comprising three structural units, and the structural formula is:

[0012]

[0013] Wherein, m, n, and p are all positive integers, m:n=(1-10):1, for example, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1; p<m; and the total average molecular weight of the ligand copolymer is 1000-100000.

[0014] Furthermore, the mass ratio of the polymer microspheres to the immobilized ligand is 1:(0.1-1), for example, 1:0.1, 1:0.3, 1:0.6, 1:0.9.

[0015] The present invention also provides a method for preparing the above-mentioned adsorbent for removing low-density lipoprotein in blood, comprising the following steps:

[0016] The polymer microspheres, solvent, epichlorohydrin, ligands coupled with iminobisethylsulfonic acid, hydroxyl and carboxyl groups, and sodium hydroxide are uniformly mixed and reacted at 25-75° C. for 2-12 hours to obtain cellulose microspheres coupled with ligands, i.e., the low-density lipoprotein adsorbent.

[0017] Furthermore, the mass ratio of the polymer microspheres to the ligand is 1:(0.1-1), for example, 1:0.3, 1:0.5, 1:0.8, 1:0.9; the mass ratio of epichlorohydrin to the ligand is 1:(2-10), for example, 1:3, 1:8.

[0018] Furthermore, the concentration of sodium hydroxide in the mixed system is 0.1-1 mol / L.

[0019] Furthermore, the preparation method of the ligand coupled with iminodiethanesulfonic acid, hydroxyl and carboxyl comprises the following steps:

[0020] S1: vinyl acetate monomer, acrylic acid monomer, initiator and solvent are uniformly mixed, and free radical polymerization is initiated at 50-80° C. The polymerization reaction is terminated to obtain a vinyl acetate-acrylic acid copolymer solution;

[0021] S2: adding thionyl chloride to the copolymer solution obtained in step S1 under ice bath conditions to obtain a partially chlorinated vinyl acetate-acrylic acid copolymer solution;

[0022] S3: adding N-(2-aminoethyl)-2-iminodiethanesulfonic acid to the copolymer solution obtained in step S2, and reacting for 1 to 3 hours at 0 to 30° C. to obtain a vinyl acetate-acrylic acid-diethanesulfonic acid acrylamide copolymer solution;

[0023] S4: adding sodium hydroxide solution to the copolymer solution obtained in step S3, reacting at 40-90° C. overnight to obtain a polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide copolymer solution;

[0024] S5: adding an anti-solvent to the copolymer solution obtained in step S4 to precipitate the polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide copolymer, and drying to obtain polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide copolymer powder, i.e., a ligand coupled with iminodiethylsulfonic acid, hydroxyl, and carboxyl groups.

[0025] The changes in the reaction products involved in the preparation process of the ligand coupled with iminobisethanesulfonic acid, hydroxyl and carboxyl groups are as follows:

[0026]

[0027] Furthermore, the molar ratio of acrylic acid monomer to vinyl acetate monomer in S1 is (1-10):1, for example, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1.

[0028] Furthermore, the molar ratio of thionyl chloride to acrylic acid monomer added in S2 is (0.1-1):1, for example, 0.3:1, 0.5:1, 0.8:1, 0.9:1.

[0029] Furthermore, the molar amount of N-(2-aminoethyl)-2-iminobisethanesulfonic acid added in S3 is 1 to 1.2 times the molar amount of thionyl chloride added in S2, preferably an equimolar amount with the thionyl chloride.

[0030] Furthermore, the concentration of the sodium hydroxide solution added in S4 is 0.1-2 mol / L, and the volume of the added sodium hydroxide solution is 10%-50% of the volume of the vinyl acetate-acrylic acid-diethylsulfonic acid acrylamide copolymer solution.

[0031] For free radical polymerization, chain termination is divided into coupling termination and disproportionation termination. The amount of initiator used has a certain relationship with the final polymerization degree of the obtained polymer. The amount of initiator used in this application is 0.1% to 1% of the total weight of the monomer.

[0032] Furthermore, the initiator described in S1 is AIBN.

[0033] Furthermore, the solvent described in S1 is tetrahydrofuran, and the anti-solvent used in S5 is methanol.

[0034] Furthermore, in S5, an anti-solvent with a temperature lower than 5° C. is used to precipitate the copolymer.

[0035] The surface of the adsorbent prepared by the present invention carries a large amount of negative charge, which is conducive to adsorption with LDL and VLDL with positive charge on the surface through electrostatic attraction, and has no obvious adsorption effect on beneficial components in the blood such as high-density lipoprotein. The apolipoprotein of LDL and VLDL is mainly ApoB, and a large amount of basic amino acid residues such as lysine, arginine and histidine contained in ApoB are exposed on the surface of apolipoprotein. These amino acid residues are positively charged under normal physiological pH environment, so the negatively charged ligand and LDL and VLDL can have specific adsorption due to electrostatic effect. The ligand in the present invention is similar to the chemical composition of heparin, has sulfonic acid group, hydroxyl group and carboxyl group, and has physiological properties similar to heparin, such as anticoagulation, specific binding to lipoprotein, etc. The N-(2-aminoethyl)-2-iminobisethylsulfonic acid introduced in the present invention has two sulfonic acid groups in one monomer structural unit. At the same time, since the new ligand has a longer side chain structure, the sulfonic acid group is at the outermost end of the side chain, which is beneficial to capturing lipoprotein in the blood when interacting with the blood. Therefore, the adsorption effect of LDL and VLDL is better than heparin when a smaller amount of ligand is added.

[0036] The present invention prepares LDL and VLDL adsorbents by coupling heparin-like ligands to the surface of polymer microspheres, which can achieve the effect of clearing more than 70% of low-density lipoproteins and more than 60% of very low-density lipoproteins in human blood, while the nonspecific adsorption rate of high-density lipoprotein HDL is less than 20%. DETAILED DESCRIPTION

[0037] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0038] Example 1

[0039] S1, 0.1 mol of vinyl acetate monomer and 0.9 mol of acrylic acid monomer are dissolved in a 500 ml three-necked flask filled with tetrahydrofuran, and 0.1% of the total weight of the monomers as AIBN initiator are added, and the mixture is reacted at 70° C. for 10 hours. The polymerization reaction is terminated to obtain a vinyl acetate-acrylic acid copolymer solution.

[0040] S2, placing a three-necked flask in an ice bath, adding 0.1 mol of thionyl chloride to partially chlorinate the carboxyl groups, and obtaining a partially chlorinated vinyl acetate-acrylic acid copolymer solution.

[0041] S3, raising the ambient temperature of the three-necked flask to 10° C., adding 0.1 mol of N-(2-aminoethyl)-2-iminobis(ethylenesulfonic acid) and reacting for 2 hours to obtain vinyl acetate-acrylic acid-bis(ethylenesulfonic acid) acrylamide.

[0042] S4, adding 100 ml of 0.5 M sodium hydroxide solution to the obtained vinyl acetate-acrylic acid-sulfonic acid acrylamide to hydrolyze the vinyl acetate, reacting at 50° C. overnight to obtain the final product, polyvinyl alcohol-acrylic acid-sulfonic acid acrylamide copolymer solution.

[0043] S5, pouring the obtained copolymer solution into pre-cooled methanol below 5°C to precipitate the polymer, and the precipitate is dried to form a white solid powder. The polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide copolymer is used as a ligand of a low-density lipoprotein adsorbent.

[0044] S6, take 100g of cellulose microspheres, add them into 300ml of DMF solvent, add 20g of epichlorohydrin and 70g of the above-mentioned polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide ligand and 10ml of 1M sodium hydroxide solution, react at 50°C for 12 hours, wash away the solvent and unreacted ligand with pure water, and obtain cellulose microspheres coupled with polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide ligand as a blood low-density lipoprotein adsorbent.

[0045] Embodiments 2 to 4

[0046] The difference between Examples 2 to 4 and Example 1 is that the amount of N-(2-aminoethyl)-2-iminobisethanesulfonic acid added to S3 is 0.3 mol, 0.6 mol, and 0.9 mol, respectively.

[0047] Embodiments 5 to 7

[0048] The difference between Examples 5 to 7 and Example 3 is that the masses of the ligand added to S6 are 10 g, 80 g, and 100 g, respectively.

[0049] Experimental example

[0050] In vitro blood adsorption experiment, 10 ml of patient plasma was taken to measure the concentrations of LDL, VLDL, HDL, TC, and TG before blood purification. LDL1 , C VDL1 , C HDL1 , C TC1 , C TG1 , add 1 ml of adsorbent to the plasma, shake at 37 ° C for 2 hours, take the supernatant to determine the concentrations of LDL, VLDL, HDL, TC, and TG in the purified blood LDL2 , C VLDL2 , C HDL2 , C TC2 , C TG2 , the final adsorbent removal rate is calculated as follows:

[0051] LDL clearance rate = (C LDL1 -C LDL2 ) / C LDL1 ;

[0052] VLDL clearance rate = (C VLDL1 -C VLDL2 ) / C VLDL1 ;

[0053] HDL clearance rate = (C HDL1 -C HDL2 ) / C HDL1 ;

[0054] TC clearance rate = (C TC1 -C TC2 ) / C TC1 ;

[0055] TG clearance rate = (C TG1 -C TG2 ) / C TG1 ;

[0056] The low density lipoprotein adsorbents provided in Examples 1 to 4 were used as samples to test and calculate the corresponding clearance rates, and the specific results are shown in Table 1. For comparison, the above test was performed using a heparin ligand adsorbent produced by a domestic company, and the specific results are shown in Table 1.

[0057] Table 1 The removal rate test results of the adsorption scavengers described in the examples and comparative examples

[0058]

[0059] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.

Claims

1. An adsorbent for blood purification, characterized in that: The invention comprises polymer microspheres as carriers and ligands fixed on the surface of the carriers; the ligands are chain polymers coupled with iminobisethylsulfonic acid, hydroxyl groups and carboxyl groups.

2. The adsorbent according to claim 1, characterized in that The polymer microspheres are selected from cellulose microspheres, agarose microspheres, dextran microspheres, polyvinyl alcohol microspheres, polyacrylate microspheres, polystyrene microspheres, and polyacrylic acid microspheres.

3. The adsorbent according to claim 1, characterized in that The ligand is a copolymer, comprising three structural units, and the structural formula is: Wherein, m:n=(1-10):1; p<m; and the total average molecular weight of the ligand is 1000-100000.

4. The adsorbent according to claim 1, characterized in that The mass ratio of the polymer microspheres to the immobilized ligand is 1:(0.1-1).

5. A method for preparing an adsorbent according to any one of claims 1 to 4, characterized in that: The steps include: The polymer microspheres, solvent, epichlorohydrin, ligands coupled with iminobisethylsulfonic acid, hydroxyl and carboxyl groups, and sodium hydroxide are uniformly mixed and reacted at 25-75° C. for 2-12 hours to obtain polymer microspheres coupled with ligands, i.e., the adsorbent for blood purification.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the polymer microspheres to the ligand is 1:(0.1-1); the mass ratio of the epichlorohydrin to the ligand is 1:(2-10).

7. The preparation method according to claim 5, characterized in that: The concentration of sodium hydroxide in the mixed system is 0.1-1 mol / L.

8. The preparation method according to claim 5, characterized in that: The preparation method of the ligand coupled with iminobisethanesulfonic acid, hydroxyl and carboxyl comprises the following steps: S1: Evenly mix vinyl acetate monomer, acrylic acid monomer, initiator and solvent, and initiate polymerization at 50-80° C. to obtain a vinyl acetate-acrylic acid copolymer solution; S2: adding thionyl chloride to the copolymer solution obtained in step S1 under ice bath conditions to obtain a partially chlorinated vinyl acetate-acrylic acid copolymer solution; S3: adding N-(2-aminoethyl)-2-iminodiethanesulfonic acid to the copolymer solution obtained in step S2, and reacting for 1 to 3 hours at 0 to 30° C. to obtain a vinyl acetate-acrylic acid-diethanesulfonic acid acrylamide copolymer solution; S4: adding sodium hydroxide solution to the copolymer solution obtained in step S3, reacting at 40-90° C. overnight to obtain a polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide copolymer solution; S5: adding an anti-solvent to the copolymer solution obtained in step S4 to precipitate the polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide copolymer, and drying to obtain polyvinyl alcohol-acrylic acid-diethylsulfonic acid acrylamide copolymer powder, i.e., a ligand coupled with iminodiethylsulfonic acid, hydroxyl and carboxyl groups.

9. The preparation method according to claim 5, characterized in that: The molar ratio of vinyl acetate monomer to acrylic acid monomer in S1 is 1:(1-10); The molar ratio of thionyl chloride to acrylic acid monomer added in S2 is (0.1-1):1; The molar amount of N-(2-aminoethyl)-2-iminobisethanesulfonic acid added to S3 is 1 to 1.2 times the molar amount of thionyl chloride added to S2; The concentration of the sodium hydroxide solution added in S4 is 0.1-2 mol / L, and the volume of the added sodium hydroxide solution is 10%-50% of the volume of the vinyl acetate-acrylic acid-diethylsulfonic acid acrylamide copolymer solution.

10. The preparation method according to claim 5, characterized in that: The initiator described in S1 is AIBN; The amount of initiator in S1 is 0.1% to 1% of the total weight of the monomers; The solvent described in S1 is tetrahydrofuran, and the anti-solvent used in S5 is methanol.

Citation Information

Patent Citations

  • Adsorption scavenger for removing low-density lipoprotein in blood and preparation method thereof

    CN109092261A

  • Filter membrane for removing low density lipoproteins, and preparation method thereof

    CN109647227A

  • Selective adsorbent low density lipoprotein cholesterol and method for preparing same