Recombinant collagen solution with low conductivity as well as preparation method and application thereof
By using hydroxyethylpiperazine ethane sulfonic acid and tromethamine in a specific ratio with polyethylene glycols, the method improves recombinant collagen solution quality for cosmetic applications by increasing collagen content and maintaining low conductivity.
Patent Information
- Application Number
- CN202411356973.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing methods for preparing recombinant collagen solutions result in low collagen content and high conductivity, which hinders their application, particularly in cosmetics.
A method involving the use of hydroxyethylpiperazine ethane sulfonic acid and tromethamine in a specific mass ratio to form a reconstitution solvent, combined with polyethylene glycols for precipitation, to achieve a pH range suitable for recombinant collagen dissolution, thereby increasing collagen content while maintaining low conductivity.
The method significantly enhances the recombinant collagen content in the solution while keeping conductivity low, making it suitable for cosmetic applications.
Smart Images

Figure BDA0005066728100000141 
Figure BDA0005066728100000151 
Figure BDA0005066728100000161
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of recombinant collagen processing, and in particular to a recombinant collagen solution with low electrical conductivity, and a preparation method and application thereof. Background Art
[0002] The fermentation filtrate containing recombinant collagen contains recombinant collagen and high concentration of salt ions. It is usually necessary to desalinate the fermentation filtrate containing recombinant collagen to obtain the recombinant collagen precipitate for subsequent application.
[0003] When the recombinant collagen precipitate is used for subsequent applications, the recombinant collagen precipitate needs to be redissolved to form a recombinant collagen solution for application. However, currently, when the recombinant collagen precipitate is redissolved to form a recombinant collagen solution, the content of recombinant collagen dissolved in the recombinant collagen solution may be low, and the conductivity of the formed recombinant collagen solution may increase too much, which is not conducive to the application of the recombinant collagen solution. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the embodiments of the present application includes providing a recombinant collagen solution with low conductivity and a preparation method and application thereof, so as to prepare a recombinant collagen solution with a high content of recombinant collagen and a conductivity that does not increase too much.
[0005] In a first aspect, an embodiment of the present application provides a method for preparing a recombinant collagen solution with low conductivity, comprising: dissolving a recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazine ethane sulfonic acid and tromethamine, and the mass ratio of hydroxyethylpiperazine ethane sulfonic acid to tromethamine is 0.3-8.3:1.
[0006] The present application adopts hydroxyethylpiperazine ethane sulfonic acid and tromethamine in a certain mass ratio to form a reconstitution solvent, which can achieve a pH range suitable for the dissolution of recombinant collagen precipitation, so as to increase the dissolution amount of recombinant collagen in the recombinant collagen solution, while ensuring that the conductivity of the recombinant collagen solution does not increase significantly.
[0007] In some embodiments of the present application, the mass ratio of hydroxyethylpiperazineethane sulfonic acid to tromethamine is 1-3:1.
[0008] The present application further adjusts hydroxyethylpiperazine ethane sulfonic acid and tromethamine in a more suitable mass ratio to form a reconstitution solvent, which can further achieve a pH range that is more suitable for the precipitation and dissolution of recombinant collagen, further increase the amount of recombinant collagen dissolved in the recombinant collagen solution, and at the same time ensure that the conductivity of the recombinant collagen solution does not increase significantly.
[0009] In a second aspect, the present application provides a method for preparing a recombinant collagen solution with low conductivity, comprising:
[0010] (1) mixing the fermentation filtrate containing recombinant collagen with a collagen precipitant for precipitation, performing solid-liquid separation and removing the supernatant to obtain a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 20%-30% polyethylene glycol-8000, 9%-15% polyethylene glycol-6000, 3%-5% polyethylene glycol-4000 and 50%-60% water;
[0011] (2) dissolving the recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazineethanesulfonic acid and tromethamine, and the mass ratio of hydroxyethylpiperazineethanesulfonic acid to tromethamine is 0.3-8.3:1.
[0012] The present application adopts polyethylene glycol-8000, polyethylene glycol-6000 and polyethylene glycol-4000 in a certain weight ratio to form a collagen precipitant, which can efficiently precipitate the recombinant collagen in the fermentation filtrate containing recombinant collagen and remove salt ions, so that the recombinant collagen solution formed by subsequent re-dissolution has a lower conductivity; at the same time, hydroxyethylpiperazineethane sulfonic acid and tromethamine are used in a certain mass ratio to form a re-dissolution solvent, which can reach a pH range suitable for the precipitation and dissolution of recombinant collagen, so as to increase the solubility of recombinant collagen in the recombinant collagen solution, while ensuring that the conductivity of the recombinant collagen solution does not increase too much, so that the recombinant collagen solution maintains a low conductivity.
[0013] In some embodiments of the present application, the pH value of the reconstitution solvent is 6.8-7.5.
[0014] The present application uses a redissolution solvent with a pH value of 6.8-7.5, which is suitable for dissolving recombinant collagen precipitates and helps to increase the amount of recombinant collagen dissolved in the recombinant collagen solution formed after dissolution.
[0015] In some embodiments of the present application, the fermentation filtrate of the recombinant collagen is mixed with the collagen precipitant in a volume ratio of 2:3-5.
[0016] The present application adopts a method of mixing the fermentation filtrate containing recombinant collagen with a collagen precipitant in a certain volume ratio, which can improve the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing recombinant collagen to a certain extent, and further efficiently remove salt ions so that the recombinant collagen solution formed by subsequent re-dissolution has a further lower conductivity.
[0017] In some embodiments of the present application, the Pichia pastoris fermentation filtrate containing recombinant collagen is mixed with a collagen precipitant and stirred at 35-38° C. for 20-30 hours.
[0018] The present application uses a fermentation filtrate containing recombinant collagen and a collagen precipitant to precipitate at an appropriate temperature, which can improve the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing recombinant collagen to a certain extent, and further efficiently remove salt ions so that the recombinant collagen solution formed by subsequent re-dissolution has a further lower conductivity.
[0019] In some embodiments of the present application, the reconstitution solvent includes, by mass percentage, 5%-9.5% glycerol, 0.1%-0.5% hydroxyethylpiperazineethane sulfonic acid, 0.06%-0.3% tromethamine, 0.01%-0.03% Tween-20, 0.003%-0.006% ethylenediaminetetraacetic acid and 90%-94.5% water.
[0020] In a third aspect, the present application provides a method for preparing a recombinant collagen solution with low conductivity, comprising:
[0021] (1) mixing a fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3-5, mixing and precipitating at 35-38° C., and removing the supernatant by solid-liquid separation to obtain a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 20%-30% polyethylene glycol-8000, 9%-15% polyethylene glycol-6000, 3%-5% polyethylene glycol-4000 and 50%-60% water;
[0022] (2) dissolving the recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazineethanesulfonic acid and tromethamine, and the mass ratio of hydroxyethylpiperazineethanesulfonic acid to tromethamine is 1-3:1.
[0023] The present application uses polyethylene glycol-8000, polyethylene glycol-6000 and polyethylene glycol-4000 in a certain weight ratio to form a collagen precipitant, and at the same time, the fermentation filtrate containing recombinant collagen is mixed with the collagen precipitant in a certain volume ratio, and precipitated at an appropriate temperature, so that the recombinant collagen in the fermentation filtrate containing recombinant collagen can be further efficiently precipitated and the salt ions can be removed, so that the recombinant collagen solution formed by subsequent re-dissolution has a lower conductivity; at the same time, hydroxyethylpiperazineethane sulfonic acid and tromethamine are used in a certain mass ratio to form a re-dissolution solvent, which can reach a pH range suitable for the precipitation and dissolution of recombinant collagen, so as to increase the solubility of recombinant collagen in the recombinant collagen solution, while ensuring that the conductivity of the recombinant collagen solution does not increase too much, so that the recombinant collagen solution maintains a low conductivity.
[0024] In a fourth aspect, an embodiment of the present application provides a recombinant collagen solution with low conductivity prepared by the preparation method provided in the first aspect, the second aspect or the third aspect.
[0025] The recombinant collagen solution prepared by the above-mentioned preparation method in the present application has a high content of recombinant collagen and a low conductivity.
[0026] In a fifth aspect, an embodiment of the present application provides a use of a recombinant collagen solution with low conductivity as provided in the fourth aspect in the preparation of cosmetics.
[0027] The recombinant collagen solution provided in the present application has a high recombinant collagen content and a low electrical conductivity, which is conducive to application in the preparation of cosmetics. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0029] Currently, when recombinant collagen precipitate is redissolved to form a recombinant collagen solution, the content of dissolved recombinant collagen in the recombinant collagen solution may be low, and the conductivity of the formed recombinant collagen solution may increase too much, which is not conducive to the application of the recombinant collagen solution.
[0030] In order to improve the problem that the content of dissolved recombinant collagen in the current recombinant collagen solution is low and the conductivity is too high, the embodiment of the present application provides a method for preparing a recombinant collagen solution with low conductivity, comprising: dissolving a recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazineethanesulfonic acid and tromethamine, and the mass ratio of hydroxyethylpiperazineethanesulfonic acid to tromethamine is 0.3-8.3:1.
[0031] By combining hydroxyethylpiperazineethane sulfonic acid and tromethamine in a certain mass ratio to form a reconstitution solvent, a pH range suitable for the dissolution of recombinant collagen precipitation can be achieved, so as to increase the amount of recombinant collagen dissolved in the recombinant collagen solution. Moreover, when the hydroxyethylpiperazineethane sulfonic acid and tromethamine are combined to form a suitable pH range, the conductivity of the obtained reconstitution solvent is low, so as to ensure that the conductivity of the recombinant collagen solution does not increase too much.
[0032] In some embodiments of the present application, the mass ratio of hydroxyethylpiperazineethane sulfonic acid to tromethamine is 1-3: 1. As an example, the mass ratio of hydroxyethylpiperazineethane sulfonic acid to tromethamine can be, but is not limited to, 0.3: 1, 0.5: 1, 0.8: 1, 1.1: 1, 1.4: 1, 1.7: 1, 2: 1, 2.5: 1, 2.8: 1, 3: 1, 3.3: 1, 3.5: 1, 3.8: 1, 4: 1, 4.3: 1, 4.5: 1, 4.8: 1, 5: 1, 5.3: 1, 5.5: 1, 5.8: 1, 6: 1, 6.3: 1, 6.5: 1, 6.8: 1, 7: 1, 7.3: 1, 7.5: 1, 7.8: 1, 8: 1, 8.3: 1. Further adjusting hydroxyethylpiperazine ethane sulfonic acid and tromethamine to a more suitable mass ratio to form a reconstitution solvent can further achieve a pH range that is more suitable for the precipitation and dissolution of recombinant collagen, further increase the amount of recombinant collagen dissolved in the recombinant collagen solution, and at the same time ensure that the conductivity of the recombinant collagen solution does not increase significantly.
[0033] The present application embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising:
[0034] (1) mixing the fermentation filtrate containing recombinant collagen with a collagen precipitant for precipitation, performing solid-liquid separation and removing the supernatant to obtain a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 20%-30% polyethylene glycol-8000, 9%-15% polyethylene glycol-6000, 3%-5% polyethylene glycol-4000 and 50%-60% water;
[0035] (2) dissolving the recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazineethanesulfonic acid and tromethamine, and the mass ratio of hydroxyethylpiperazineethanesulfonic acid to tromethamine is 0.3-8.3:1.
[0036] Polyethylene glycol-8000, polyethylene glycol-6000 and polyethylene glycol-4000 are mixed in a certain weight ratio to form a collagen precipitant, so that the recombinant collagen in the fermentation filtrate containing the recombinant collagen can be efficiently precipitated and salt ions can be removed, so that the recombinant collagen solution formed by subsequent redissolution has a lower conductivity; at the same time, hydroxyethylpiperazineethanesulfonic acid and tromethamine are mixed in a certain mass ratio to form a redissolution solvent, so that a pH range suitable for the precipitation and dissolution of the recombinant collagen can be achieved, so as to increase the dissolution amount of the recombinant collagen in the recombinant collagen solution, and when the hydroxyethylpiperazineethanesulfonic acid and tromethamine are mixed in a suitable pH range, the conductivity of the obtained redissolution solvent is low, so as to ensure that the conductivity of the recombinant collagen solution does not increase too much, so that the recombinant collagen solution maintains a low conductivity.
[0037] As an example, the weight percentage of polyethylene glycol-8000 in the collagen precipitant may be, but is not limited to, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%. The weight percentage of polyethylene glycol-6000 in the collagen precipitant may be, but is not limited to, 9%, 10%, 11%, 12%, 13%, 14%, 15%. The weight percentage of polyethylene glycol-4000 in the collagen precipitant may be, but is not limited to, 3%, 3.5%, 4%, 4.5%, 5%. Polyethylene glycol-8000, polyethylene glycol-6000 and polyethylene glycol-4000 are combined in an appropriate weight ratio to form a collagen precipitant, which can achieve rapid and efficient separation and precipitation of recombinant collagen from the fermentation filtrate of recombinant collagen containing a high concentration of salt ions. The operation is convenient and economical, and the recombinant collagen solution formed by subsequent re-dissolution has a lower conductivity.
[0038] In some embodiments of the present application, the pH value of the reconstitution solvent is 6.8-7.5. As an example, the pH value of the reconstitution solvent can be, but is not limited to, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5. The use of a reconstitution solvent with a pH value of 6.8-7.5 is suitable for dissolving the recombinant collagen precipitate, which is conducive to increasing the amount of recombinant collagen dissolved in the recombinant collagen solution formed after dissolution.
[0039] In some embodiments of the present application, the fermentation filtrate of recombinant collagen is mixed with a collagen precipitant at a volume ratio of 2:3-5. As an example, the fermentation filtrate of recombinant collagen and the collagen precipitant can be mixed with, but not limited to, a volume ratio of 2:3, 2:4, 2:5. By mixing the fermentation filtrate containing recombinant collagen with the collagen precipitant at a certain volume ratio, the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing the recombinant collagen can be improved to a certain extent, and the salt ions can be further efficiently removed, so that the recombinant collagen solution formed by the subsequent redissolution further has a lower conductivity.
[0040] In some embodiments of the present application, the fermentation filtrate of Pichia pastoris containing recombinant collagen is mixed with a collagen precipitant and stirred at 35-38°C for 20-30h. As an example, the fermentation filtrate of Pichia pastoris containing recombinant collagen and the collagen precipitant can be stirred at, but not limited to, 35°C, 36°C, 37°C, and 38°C. The precipitation of the fermentation filtrate containing recombinant collagen and the collagen precipitant at a suitable temperature can improve the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing recombinant collagen to a certain extent, and further efficiently remove salt ions, so that the recombinant collagen solution formed by subsequent redissolution has a lower conductivity.
[0041] In some embodiments of the present application, the reconstitution solvent includes, by mass percentage, 5%-9.5% glycerol, 0.1%-0.5% hydroxyethylpiperazineethane sulfonic acid, 0.06%-0.3% tromethamine, 0.01%-0.03% Tween-20, 0.003%-0.006% ethylenediaminetetraacetic acid and 90%-94.5% water.
[0042] As an example, the weight percentage of hydroxyethylpiperazineethanesulfonic acid in the reconstitution solvent may be, but is not limited to, 0.1%, 0.12%, 0.15%, 0.18%, 0.2%, 0.22%, 0.24%, 0.25%, 0.28%, 0.3%, 0.32%, 0.35%, 0.38%, 0.4%, 0.42%, 0.44%, 0.45%, 0.48%, 0.5%. The weight percentage of tromethamine in the reconstitution solvent may be, but is not limited to, 0.06%, 0.08%, 0.1%, 0.12%, 0.14%, 0.15%, 0.18%, 0.2%, 0.22%, 0.24%, 0.25%, 0.28%, 0.3%.
[0043] The present application embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising:
[0044] (1) mixing a fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3-5, mixing and precipitating at 35-38° C., and removing the supernatant by solid-liquid separation to obtain a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 20%-30% polyethylene glycol-8000, 9%-15% polyethylene glycol-6000, 3%-5% polyethylene glycol-4000 and 50%-60% water;
[0045] (2) dissolving the recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazineethanesulfonic acid and tromethamine, and the mass ratio of hydroxyethylpiperazineethanesulfonic acid to tromethamine is 1-3:1.
[0046] Polyethylene glycol-8000, polyethylene glycol-6000 and polyethylene glycol-4000 are mixed in a certain weight ratio to form a collagen precipitant, and fermentation filtrate containing recombinant collagen is mixed with the collagen precipitant in a certain volume ratio, and precipitation is performed at a suitable temperature, so that the recombinant collagen in the fermentation filtrate containing the recombinant collagen can be further efficiently precipitated, and salt ions can be removed, so that the recombinant collagen solution formed by subsequent redissolution has a lower conductivity; at the same time, hydroxyethylpiperazineethanesulfonic acid and tromethamine are mixed in a certain mass ratio to form a redissolution solvent, so that a pH range suitable for recombinant collagen precipitation and dissolution can be reached, so as to increase the dissolution amount of recombinant collagen in the recombinant collagen solution, and when the hydroxyethylpiperazineethanesulfonic acid and tromethamine are mixed in a suitable pH range, the conductivity of the obtained redissolution solvent is low, so as to ensure that the conductivity of the recombinant collagen solution does not increase too much, so that the recombinant collagen solution maintains a low conductivity.
[0047] The embodiment of the present application provides a recombinant collagen solution with low conductivity prepared by the above-mentioned preparation method.
[0048] The recombinant collagen solution prepared by the above preparation method has a higher content of recombinant collagen and a lower conductivity.
[0049] The embodiments of the present application provide a use of the above-mentioned recombinant collagen solution with low conductivity in the preparation of cosmetics.
[0050] The recombinant collagen solution has a high recombinant collagen content and low electrical conductivity, which is conducive to application in the preparation of cosmetics.
[0051] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0052] The fermentation filtrate containing recombinant collagen in the present application was purchased from Best Pharmaceutical (Guangzhou) Co., Ltd.
[0053] Example 1
[0054] This embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising the following steps:
[0055] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 30% polyethylene glycol-8000, 15% polyethylene glycol-6000, 5% polyethylene glycol-4000, and 50% water;
[0056] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 7.2.
[0057] The recombinant collagen solution prepared by the preparation method provided in this example is denoted as A.
[0058] Example 2
[0059] This embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising the following steps:
[0060] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 15% polyethylene glycol-8000, 7.5% polyethylene glycol-6000, 2.5% polyethylene glycol-4000, and 75% water;
[0061] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 7.2.
[0062] The recombinant collagen solution prepared by the preparation method provided in this example is denoted as B.
[0063] Example 3
[0064] This embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising the following steps:
[0065] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 50% polyethylene glycol-8000 and 50% water;
[0066] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 7.2.
[0067] The recombinant collagen solution prepared by the preparation method provided in this example is denoted as C.
[0068] Example 4
[0069] This embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising the following steps:
[0070] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 50% polyethylene glycol-6000 and 50% water;
[0071] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 7.2.
[0072] The recombinant collagen solution prepared by the preparation method provided in this example is denoted as D.
[0073] Example 5
[0074] This embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising the following steps:
[0075] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 50% polyethylene glycol-4000 and 50% water;
[0076] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 7.2.
[0077] The recombinant collagen solution prepared by the preparation method provided in this example is denoted as E.
[0078] Example 6
[0079] This embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising the following steps:
[0080] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 1:1, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 30% polyethylene glycol-8000, 15% polyethylene glycol-6000, 5% polyethylene glycol-4000, and 50% water;
[0081] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 7.2.
[0082] The recombinant collagen solution prepared by the preparation method provided in this example is denoted as F.
[0083] Example 7
[0084] This embodiment provides a method for preparing a recombinant collagen solution with low conductivity, comprising the following steps:
[0085] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 25° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 30% polyethylene glycol-8000, 15% polyethylene glycol-6000, 5% polyethylene glycol-4000, and 50% water;
[0086] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 7.2.
[0087] The recombinant collagen solution prepared by the preparation method provided in this example is denoted as G.
[0088] Comparative Example 1
[0089] This comparative example provides a method for preparing a recombinant collagen solution, comprising the following steps:
[0090] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 30% polyethylene glycol-8000, 15% polyethylene glycol-6000, 5% polyethylene glycol-4000, and 50% water;
[0091] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.24% hydroxyethylpiperazineethanesulfonic acid, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 5.
[0092] The recombinant collagen solution prepared by the preparation method provided in this comparative example is recorded as M1.
[0093] Comparative Example 2
[0094] This comparative example provides a method for preparing a recombinant collagen solution, comprising the following steps:
[0095] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 30% polyethylene glycol-8000, 15% polyethylene glycol-6000, 5% polyethylene glycol-4000, and 50% water;
[0096] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.12% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 10.
[0097] The recombinant collagen solution prepared by the preparation method provided in this comparative example is recorded as M2.
[0098] Comparative Example 3
[0099] This comparative example provides a method for preparing a recombinant collagen solution, comprising the following steps:
[0100] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 30% polyethylene glycol-8000, 15% polyethylene glycol-6000, 5% polyethylene glycol-4000, and 50% water;
[0101] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.05% hydroxyethylpiperazineethanesulfonic acid, 0.4% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and the pH value of the reconstitution solvent is 8.5.
[0102] The recombinant collagen solution prepared by the preparation method provided in this comparative example is recorded as M3.
[0103] Comparative Example 4
[0104] This comparative example provides a method for preparing a recombinant collagen solution, comprising the following steps:
[0105] (1) mixing a Pichia pastoris fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3, stirring and mixing at 37° C. for 24 hours, centrifuging, removing the supernatant, and obtaining a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 30% polyethylene glycol-8000, 15% polyethylene glycol-6000, 5% polyethylene glycol-4000, and 50% water;
[0106] (2) Dissolve 1 g of recombinant collagen precipitate in 1000 mL of a reconstitution solvent, stir at 4°C for 24 h to fully dissolve, and obtain a 1 mg / mL recombinant collagen solution; wherein the reconstitution solvent comprises, by mass percentage, 5% glycerol, 0.08% tromethamine, 0.01% Tween-20, 0.003% ethylenediaminetetraacetic acid, and 94.5% water; and adjust the pH value of the reconstitution solvent to 7.2 using 1% sodium hydroxide solution.
[0107] The recombinant collagen solution prepared by the preparation method provided in this comparative example is recorded as M4.
[0108] The preparation methods of the recombinant collagen solutions provided in Examples 1-7 and Comparative Examples 1-4 are shown in Table 1.
[0109] Table 1 Preparation method of recombinant collagen solution
[0110]
[0111]
[0112]
[0113] Note: “ / ” in the table means that the component is not included.
[0114] Test Example 1
[0115] In this test example, the protein content of the recombinant collagen solution AG prepared in Examples 1-7 and the recombinant collagen solution M1-M4 prepared in Comparative Examples 1-4 was determined by spectrophotometry. The specific method is as follows:
[0116] Pipette 20 μL of standard protein stock solution, water (blank control group) and each recombinant collagen solution sample into a 96-well plate, add 200 μL of BCA reagent to each well, shake gently, and incubate in a 37°C oven for 45 minutes. After incubation, cool to room temperature, and use the blank as a control to measure the absorbance of each well at 562nm on an ELISA reader. Draw a standard curve based on the absorbance values of the standard protein of the series concentration, and calculate the protein content in the standard curve based on the absorbance values of each recombinant collagen solution sample. The results are shown in Table 2.
[0117] Table 2 Protein content in recombinant collagen solution
[0118] Recombinant collagen solution Protein content (mg / mL) A 1.00 B 1.00 C 1.00 D 1.00 E 1.00 F 1.00 G 1.00 M1 0.86 M2 0.45 M3 0.31 M4 1.00
[0119] It can be seen from the results in Table 2 that, compared with the recombinant collagen solution AG prepared in Examples 1-7 and the recombinant collagen solution M1-M3 prepared in Comparative Examples 1-3, the protein content of the recombinant collagen solution AG prepared in Examples 1-7 is increased by 16.3%, 122.2% and 222.6% respectively compared with the recombinant collagen solution M1-M3 prepared in Comparative Examples 1-3. This indicates that the reconstitution solvent formed by combining hydroxyethylpiperazineethanesulfonic acid and tromethamine in an appropriate mass ratio in Examples 1-7 of the present application can reach a pH range suitable for the dissolution of recombinant collagen precipitation, and can effectively increase the amount of recombinant collagen dissolved in the recombinant collagen solution.
[0120] Test Example 2
[0121] In this test example, the conductivity of each reconstitution solvent and the reconstituted collagen solution was measured using a conductivity meter for the reconstituted collagen solution AG prepared in Examples 1-7 and the reconstituted collagen solution M1-M4 prepared in Comparative Examples 1-4. The specific method is as follows:
[0122] 100 mL of each reconstitution solvent and each recombinant collagen solution were taken and placed in a 25°C oven to balance the temperature. After the solution temperature stabilized, it was placed in a conductivity probe for conductivity measurement. The results are shown in Table 3.
[0123] Table 3 Conductivity of recombinant collagen solution
[0124]
[0125] It can be seen from the results in Table 3 that the conductivity of the reconstitution solvents configured in Examples 1-7 and Comparative Examples 1-3 is relatively low, and the conductivity of the recombinant collagen solution A prepared in Example 1 and the recombinant collagen solutions M1-M3 prepared in Comparative Examples 1-3 is relatively low. However, the protein content in the recombinant collagen solution A prepared in Example 1 is much higher than the protein content in the recombinant collagen solutions M1-M3. This indicates that the present application uses a reconstitution solvent formed by combining hydroxyethylpiperazineethane sulfonic acid and tromethamine in a suitable mass ratio to achieve a pH range suitable for the dissolution of recombinant collagen precipitation, thereby increasing the amount of recombinant collagen dissolved in the recombinant collagen solution while obtaining a low conductivity reconstitution solvent, which can ensure that the conductivity of the recombinant collagen solution does not increase too much.
[0126] Comparing the recombinant collagen solution A prepared in Example 1 and the recombinant collagen solution M4 prepared in Comparative Example 4, the reconstitution solvent in Comparative Example 4 was adjusted to pH 7.2 by using sodium hydroxide. Although the protein content in the recombinant collagen solution M4 reached 1.00 mg / mL, the conductivity of the reconstitution solvent was relatively high, which increased the conductivity of the recombinant collagen solution M4 too much. This shows that the reconstitution solvent formed by combining hydroxyethylpiperazineethanesulfonic acid and tromethamine in an appropriate mass ratio in the present application can not only increase the amount of recombinant collagen dissolved in the recombinant collagen solution, but also the conductivity of the obtained reconstitution solvent is relatively low, and the conductivity of the recombinant collagen solution can be ensured not to increase too much.
[0127] Comparing the recombinant collagen solution A prepared in Example 1 and the recombinant collagen solution BE prepared in Examples 2-5, the conductivity of the recombinant collagen solution BE is too high than that of A. It is explained that the present application adopts polyethylene glycol-8000, polyethylene glycol-6000 and polyethylene glycol-4000 in a suitable weight ratio to form a collagen precipitant, which can efficiently precipitate the recombinant collagen in the fermentation filtrate containing recombinant collagen and remove salt ions, so that the recombinant collagen solution formed by subsequent redissolution has a lower conductivity; at the same time, hydroxyethylpiperazineethanesulfonic acid and tromethamine are used in a suitable mass ratio to form a redissolution solvent, which can ensure that the conductivity of the recombinant collagen solution does not increase too much on the basis of increasing the amount of recombinant collagen dissolved in the recombinant collagen solution, so that the recombinant collagen solution maintains a low conductivity.
[0128] Comparing the recombinant collagen solution A prepared in Example 1 and the recombinant collagen solution F prepared in Example 6, the conductivity of the recombinant collagen solution F is higher than that of A. This indicates that the present application uses a fermentation filtrate containing recombinant collagen and a collagen precipitant mixed in an appropriate volume ratio, which can improve the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing recombinant collagen to a certain extent, and further efficiently remove salt ions, so that the recombinant collagen solution formed by subsequent redissolution has a further lower conductivity.
[0129] Comparing the recombinant collagen solution A prepared in Example 1 and the recombinant collagen solution G prepared in Example 7, the conductivity of the recombinant collagen solution G is higher than that of A to a certain extent. This shows that the present application uses the fermentation filtrate containing recombinant collagen and the collagen precipitant to precipitate at a suitable temperature, which can improve the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing recombinant collagen to a certain extent, and further efficiently remove salt ions, so that the recombinant collagen solution formed by subsequent redissolution has a lower conductivity.
[0130] Test Example 3
[0131] This test example measures the precipitation rate of the recombinant collagen precipitate obtained in Examples 1-7 and Comparative Examples 1-4. The specific method is as follows:
[0132] Take the above recombinant collagen precipitates, use vacuum freeze drying for 48 hours, remove all water, weigh them, and calculate the protein precipitation rate according to the following formula:
[0133] Protein precipitation rate (%) = m / (C×V)×100
[0134] in:
[0135] m: weight of recombinant collagen precipitate, g;
[0136] C: Concentration of recombinant collagen in Pichia fermentation filtrate, 10.25 mg / mL;
[0137] V: volume of Pichia fermentation filtrate, 1L.
[0138] The results are shown in Table 4.
[0139] Table 4 Recombinant collagen precipitation rate
[0140]
[0141]
[0142] As shown in Table 4, compared with the recombinant collagen precipitates obtained in Example 1 and Example 2-5, the precipitation rates of the recombinant collagen obtained in Example 1 were increased by 149.4%, 40.6%, 267.7%, and 45.9%, respectively, compared with those in Example 2-5. This indicates that the present application uses polyethylene glycol-8000, polyethylene glycol-6000, and polyethylene glycol-4000 in a suitable weight ratio to form a collagen precipitant, which can achieve rapid and efficient separation and precipitation of recombinant collagen from the fermentation filtrate of recombinant collagen containing a high concentration of salt ions, and the operation is convenient and economical, which is conducive to the subsequent reconstitution The recombinant collagen solution formed has a lower conductivity.
[0143] Comparing the recombinant collagen precipitates obtained in Example 1 and Example 6, the recombinant collagen precipitation rate obtained in Example 1 was increased by 24.1% compared with that in Example 6. This indicates that the present application uses a fermentation filtrate containing recombinant collagen and a collagen precipitant mixed in an appropriate volume ratio, which can improve the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing the recombinant collagen to a certain extent, and further efficiently remove salt ions.
[0144] Comparing the recombinant collagen precipitates obtained in Example 1 and Example 7, the precipitation rate of the recombinant collagen obtained in Example 1 was increased by 40.5% compared with that in Example 6. This indicates that the present application uses the fermentation filtrate containing recombinant collagen and the collagen precipitant to precipitate at a suitable temperature, which can effectively improve the precipitation efficiency of the recombinant collagen in the fermentation filtrate containing the recombinant collagen to a certain extent, and further efficiently remove salt ions.
[0145] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
Claims
1. A method for preparing a recombinant collagen solution with low conductivity, characterized in that: The preparation method comprises: The recombinant collagen precipitate is dissolved in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazineethane sulfonic acid and tromethamine, and the mass ratio of the hydroxyethylpiperazineethane sulfonic acid to tromethamine is 0.3-8.3:
1.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the hydroxyethylpiperazineethane sulfonic acid to tromethamine is 1-3:
1.
3. A method for preparing a recombinant collagen solution with low conductivity, characterized in that: The preparation method comprises: (1) mixing the fermentation filtrate containing recombinant collagen with a collagen precipitant for precipitation, performing solid-liquid separation and removing the supernatant to obtain a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 20%-30% polyethylene glycol-8000, 9%-15% polyethylene glycol-6000, 3%-5% polyethylene glycol-4000 and 50%-60% water; (2) dissolving the recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazine ethane sulfonic acid and tromethamine, and the mass ratio of the hydroxyethylpiperazine ethane sulfonic acid to tromethamine is 0.3-8.3:
1.
4. The preparation method according to any one of claims 1 to 3, characterized in that The pH value of the reconstitution solvent is 6.8-7.
5.
5. The preparation method according to claim 3, characterized in that: The fermentation filtrate of the recombinant collagen is mixed with the collagen precipitant in a volume ratio of 2:3-5.
6. The preparation method according to claim 3, characterized in that: The Pichia fermentation filtrate containing the recombinant collagen is mixed with the collagen precipitant and stirred at 35-38° C. for 20-30 hours.
7. The preparation method according to any one of claims 1 to 3, characterized in that: The reconstitution solvent comprises, by mass percentage, 5%-9.5% glycerol, 0.1%-0.5% hydroxyethylpiperazineethanesulfonic acid, 0.06%-0.3% tromethamine, 0.01%-0.03% Tween-20, 0.003%-0.006% ethylenediaminetetraacetic acid and 90%-94.5% water.
8. A method for preparing a recombinant collagen solution with low conductivity, characterized in that: The preparation method comprises: (1) mixing a fermentation filtrate containing recombinant collagen with a collagen precipitant in a volume ratio of 2:3-5, mixing and precipitating at 35-38° C., and removing the supernatant by solid-liquid separation to obtain a recombinant collagen precipitate; wherein the collagen precipitant comprises, by weight percentage, 20%-30% polyethylene glycol-8000, 9%-15% polyethylene glycol-6000, 3%-5% polyethylene glycol-4000 and 50%-60% water; (2) dissolving the recombinant collagen precipitate in a reconstitution solvent to obtain a recombinant collagen solution; wherein the reconstitution solvent comprises hydroxyethylpiperazine ethane sulfonic acid and tromethamine, and the mass ratio of the hydroxyethylpiperazine ethane sulfonic acid to tromethamine is 1-3:
1.
9. A recombinant collagen solution with low conductivity prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the recombinant collagen solution with low conductivity as claimed in claim 9 in the preparation of cosmetics.
Citation Information
Patent Citations
Compounds useful as modulators of trpm8
CN108473484A
Toning lotion composition with effects of improving skin color and brightening skin and preparation method thereof
CN113786378A
Long-acting collagen fiber and preparation method thereof
CN116103776A
Novel process for solubilizing protein from a proteinaceous material and compositions thereof
US20090104173A1
Process for the purification of TNFR:fc fusion protein
US20170152298A1
Cited By
Recombinant collagen solution with low conductivity as well as preparation method and application thereof
CN120623317A