Organic oxide adsorbent as well as preparation method and application thereof

By preparing 13X molecular sieves with a high silicon-to-aluminum ratio and performing surface modifications, the problems of low adsorption capacity and poor selectivity of molecular sieves are solved, and efficient adsorption and selectivity improvement of organic oxides are achieved, which is suitable for hydrocarbon products with various carbon numbers. removal.

CN118719031AActive Publication Date: 2024-10-01CHINA ENERGY GRP NINGXIA COAL IND CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410976169.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-01
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

Existing molecular sieves have low adsorption capacity, poor selectivity and narrow application range for organic oxides in hydrocarbons, making it difficult to effectively remove organic oxygen compounds in coal Fischer-Tropsch synthesis or petroleum cracking products.

Method used

A 13X molecular sieve with a high silicon-to-aluminum ratio is prepared by controlling the pH value and a two-stage hydrothermal crystallization treatment, and performs organic silicon coupling agent reaction and copper salt and titanium precursor impregnation treatment on its surface to improve the dispersion and adsorption site of the adsorbent. points to form high-performance organic oxide adsorbents.

Benefits of technology

It achieves high-efficiency adsorption and improved selectivity of organic oxides, and is suitable for the removal of organic oxides in Fischer-Tropsch synthesis alkene products and hydrocarbon fuels, significantly improving the performance of the adsorbent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004954577230000121
    Figure BDA0004954577230000121
  • Figure BDA0004954577230000132
    Figure BDA0004954577230000132
Patent Text Reader

Abstract

The invention provides an organic oxide adsorbent and a preparation method and application thereof, and the preparation method comprises the following steps: preparing a seed crystal through pH value control and two-stage crystallization process, and then preparing a 13X molecular sieve with high silica-alumina ratio, excellent specific surface area and pore capacity through aging treatment and hydrothermal crystallization treatment; then the surface and the structure of the 13X molecular sieve are further modified, organic silicon is introduced into the 13X molecular sieve through reaction with an organic silicon coupling agent and calcination treatment, the dispersity and the stability of the adsorbent are improved, and adsorption sites are increased through copper salt solution dipping treatment, titanium precursor dipping treatment and secondary calcination treatment; the adsorption capacity and selectivity of the adsorbent to organic oxides are improved, the adsorbent with excellent adsorption performance to the organic oxides is obtained, and the problems that in the prior art, molecular sieves are low in adsorption capacity to the organic oxides in hydrocarbons, poor in selective adsorption performance to the organic oxides and narrow in application range are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adsorption materials, and in particular to an organic oxide adsorbent and a preparation method and application thereof. Background Art

[0002] Adsorption separation has been widely used in petroleum cracking and refinery catalytic cracking. At present, the research on adsorption separation process is mainly applied to the removal of oxygenates in C4 and above hydrocarbons by adsorption. In addition, the hydrocarbon products of coal through Fischer-Tropsch synthesis have different carbon number distributions. The molecular weight and molecular structure of oxygenates in products with different carbon numbers are very different. Therefore, there is no adsorbent that is generally used for oxygenates in products with different carbon numbers. Molecular sieve is a kind of aluminosilicate, which has the characteristics of rich pore system, large specific surface area and good thermal stability. It is considered to be the preferred adsorbent material for removing oxygenates from olefins. Among them, FAU type (X, Y type) molecular sieve has a pore size of about 0.74nm, especially X type molecular sieve can better remove oxygenate impurities in olefins. It has been studied a lot and has also been used in industrial practice. However, when it is used for olefin purification, its adsorption heat is high and its adsorption capacity is weak. In addition, part of olefins will be adsorbed during the adsorption purification process. Therefore, it is of great significance to develop molecular sieve adsorbents with high adsorption capacity, high organic oxide adsorption capacity and high organic oxide adsorption selectivity. Summary of the invention

[0003] The main purpose of the present invention is to provide an organic oxide adsorbent and a preparation method and application thereof, so as to solve the problems of low adsorption capacity of molecular sieves for organic oxides in hydrocarbons, poor selective adsorption performance of organic oxides and narrow application range in the prior art.

[0004] In order to achieve the above object, according to one aspect of the present invention, a method for preparing an organic oxide adsorbent is provided, comprising the following steps:

[0005] Step S1, mixing a silicon source and water to obtain a silicon-containing material, mixing an aluminum source and water to obtain an aluminum-containing material, stirring and mixing the aluminum-containing material and the silicon-containing material to obtain a first gel-like mother liquor, adjusting the pH value of the first gel-like mother liquor to 8.5-12.5 using sodium hydroxide, and then performing two-stage hydrothermal crystallization treatment to obtain a solution containing 13X molecular sieve seed crystals; wherein the crystallization temperature of the first stage hydrothermal crystallization treatment is 20-60° C., and the crystallization temperature of the second stage hydrothermal crystallization treatment is 80-120° C.;

[0006] Step S2, subjecting the solution containing the 13X molecular sieve seed crystals to an aging treatment, and then subjecting the solution to a hydrothermal crystallization treatment at 60 to 105° C., filtering, washing, and drying the hydrothermal crystallization product to obtain the 13X molecular sieve;

[0007] Step S3, reacting 13X molecular sieve and organosilicon coupling agent in an organic alcohol solvent to obtain organosilicon-modified 13X molecular sieve, soaking the product of the first calcination treatment in a copper salt solution to obtain a 13X molecular sieve impregnated with a copper salt solution, stirring and mixing the 13X molecular sieve impregnated with the copper salt solution and a titanium precursor sol to obtain a mixture, drying the mixture and then calcining it for the second time to obtain an organic oxide adsorbent; wherein the temperature of the first calcination treatment is 400-500°C, and the temperature of the second calcination treatment is 450-550°C.

[0008] Furthermore, the silicon source is selected from one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash, and white carbon black, and the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate, and aluminum nitrate, and the weight ratio of the silicon source to the aluminum source is (0.01-1.25):1.

[0009] Preferably, in step S1, the mass fraction of the silicon source in the silicon-containing material is 2% to 50%.

[0010] Preferably, in step S1, the silicon source and water are stirred at 20-60° C. for 0.1-12 h to obtain a silicon-containing material.

[0011] Preferably, in step S1, the mass fraction of the aluminum source in the aluminum-containing material is 15% to 60%.

[0012] Preferably, in step S1, the aluminum source and water are stirred at 20 to 60° C. for 0.1 to 12 hours to obtain an aluminum-containing material.

[0013] Preferably, in step S1, the mixture is stirred and mixed at a stirring temperature of 20 to 100° C. for 0.1 to 24 hours to obtain a first gel mother solution.

[0014] Furthermore, the pH value of the first gel-like mother solution is 11.8 to 12.5.

[0015] Preferably, in step S1, the pH value of the first gel mother liquor is adjusted by adding solid sodium hydroxide or an aqueous solution of sodium hydroxide.

[0016] Furthermore, the crystallization temperature in the second stage crystallization treatment is higher than the crystallization temperature in the first stage crystallization treatment by more than 40° C., preferably, by 50 to 60° C.

[0017] Preferably, in the first hydrothermal crystallization treatment, the crystallization temperature is 40 to 60° C., and the crystallization time is 4 to 24 hours, more preferably 11 to 24 hours.

[0018] Preferably, in the second hydrothermal crystallization treatment, the crystallization temperature is 90-100° C., and the crystallization time is 6-48 h, more preferably 18-48 h.

[0019] Preferably, the molar ratio of each component in the solution containing 13X molecular sieve seeds is: SiO2 / Al2O3=(0.01-6):1, Na2O / SiO2=(0.01-4.0):1, H2O / SiO2=(1.0-50.0):1.

[0020] Furthermore, in step S2, the aging treatment is carried out under stirring conditions, the aging treatment temperature is 20 to 100° C., and the aging treatment time is 0.1 to 24 hours.

[0021] Preferably, in step S2, the time of the hydrothermal crystallization treatment is 0.1 to 36 hours.

[0022] Preferably, in step S2, the hydrothermal crystallization product is filtered and washed to neutrality, and then dried at 80-120° C. to constant weight to obtain a 13X molecular sieve.

[0023] Furthermore, in step S3, the organic silicon coupling agent is selected from one or more of methyltriethoxysilane, isopropyltrimethoxysilane, vinyltrimethoxysilane, ethyl orthosilicate, ethoxysilane, ethyl orthosilicate, and 3-aminopropyltriethoxysilane, and the organic alcohol solvent is selected from one or more of ethanol, propanol, and butanol.

[0024] Preferably, in step S3, the mass ratio of 13X molecular sieve, organic silicon coupling agent and organic alcohol solvent is 1: (0.002-0.05): (0.8-2).

[0025] Preferably, in step S3, the reaction temperature is 15-40° C., and the reaction time is 1-10 h.

[0026] Preferably, in step S3, the first calcination treatment time is 0.5 to 4 hours.

[0027] Furthermore, in step S3, the copper salt is selected from one or more of copper nitrate, copper chloride, and copper acetate.

[0028] Preferably, in step S3, the concentration of the copper salt is 0.1 to 2 mol / L, and the soaking treatment time is 6 to 48 hours.

[0029] Furthermore, in step S3, the titanium source in the titanium precursor sol is selected from one or more of tetrabutyl titanate, titanium orthosilicate or diisopropoxy diacetylacetonate titanium.

[0030] Preferably, in step S3, the titanium precursor sol is formed by mixing a titanium source, ethanol and water.

[0031] More preferably, in step S3, the titanium source, ethanol and water are stirred and mixed at 50-70° C. for 1-6 hours to form a titanium precursor sol.

[0032] More preferably, in step S3, ethanol and water are first mixed to form a mixed solvent, and then the titanium source is added and mixed.

[0033] More preferably, in step S3, the titanium source, ethanol and water are mixed in a mass ratio of 1:(3-7):(0.5-1.5).

[0034] Preferably, in step S3, the drying temperature is 90-110° C., and the drying time is 6-18 hours.

[0035] Preferably, in step S3, the second calcination treatment time is 0.5 to 4 hours.

[0036] According to another aspect of the present invention, an organic oxide adsorbent is provided, which is prepared according to the above method for preparing the organic oxide adsorbent.

[0037] According to another aspect of the present invention, there is provided use of the above organic oxide adsorbent in removing organic oxides from hydrocarbons.

[0038] Preferably, the hydrocarbon is a hydrocarbon product obtained by Fischer-Tropsch synthesis of coal, or an olefin product obtained by petroleum cracking.

[0039] Preferably, the organic oxide is selected from one or more of alcohols, aldehydes, ketones and carboxylic acids having 1 to 21 carbon atoms.

[0040] By applying the technical scheme of the present invention, a 13X molecular sieve with a high silicon-to-aluminum ratio, excellent specific surface area and pore capacity is prepared by controlling the pH value and preparing seed crystals through a two-stage crystallization process, and then through an aging treatment and a hydrothermal crystallization treatment, the prepared 13X molecular sieve has a high silicon source utilization rate and can provide more adsorption sites; then the surface and structure of the 13X molecular sieve are further modified to obtain an organic oxide adsorbent with a high silicon-to-aluminum ratio, high specific surface area and high pore capacity, and the surface and structure modification includes introducing organic silicon into the 13X molecular sieve through reaction with an organic silicon coupling agent and calcination treatment to improve the dispersibility and stability of the adsorbent, increasing the adsorption sites through copper salt solution impregnation treatment, titanium precursor impregnation treatment and secondary calcination treatment, improving the adsorption capacity and selectivity of the adsorbent for organic oxides, and obtaining an adsorbent with excellent adsorption performance for organic oxides.

[0041] The adsorbent prepared by the method of the present invention has a high silicon-to-aluminum ratio, a high specific surface area and a high pore capacity, and has excellent adsorption performance for organic oxides, and can achieve high-efficiency adsorption and removal of organic oxides in Fischer-Tropsch synthesis alkane-olefin products, hydrocarbon fuels or organic oxides in chemical products. DETAILED DESCRIPTION

[0042] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0043] As described in the background technology, the prior art of the present invention has the problems of low adsorption capacity of molecular sieves for organic oxides in hydrocarbons, poor selective adsorption performance of organic oxides, and narrow application range. In order to solve the above problems, a method for preparing an organic oxide adsorbent is provided, comprising the following steps:

[0044] Step S1, mixing a silicon source and water to obtain a silicon-containing material, mixing an aluminum source and water to obtain an aluminum-containing material, stirring and mixing the aluminum-containing material and the silicon-containing material to obtain a first gel-like mother liquor, adjusting the pH value of the first gel-like mother liquor to 8.5-12.5 using sodium hydroxide, and then performing two-stage hydrothermal crystallization treatment to obtain a solution containing 13X molecular sieve seed crystals; wherein the crystallization temperature of the first stage hydrothermal crystallization treatment is 20-60° C., and the crystallization temperature of the second stage hydrothermal crystallization treatment is 80-120° C.;

[0045] Step S2, subjecting the solution containing the 13X molecular sieve seed crystals to an aging treatment, and then subjecting the solution to a hydrothermal crystallization treatment at 60 to 105° C., filtering, washing, and drying the hydrothermal crystallization product to obtain the 13X molecular sieve;

[0046] Step S3, reacting 13X molecular sieve and organosilicon coupling agent in an organic alcohol solvent to obtain organosilicon-modified 13X molecular sieve, soaking the product of the first calcination treatment in a copper salt solution to obtain a 13X molecular sieve impregnated with a copper salt solution, stirring and mixing the 13X molecular sieve impregnated with the copper salt solution and a titanium precursor sol to obtain a mixture, drying the mixture and then calcining it for the second time to obtain an organic oxide adsorbent; wherein the temperature of the first calcination treatment is 400-500°C, and the temperature of the second calcination treatment is 450-550°C.

[0047] In order to obtain a high-performance organic oxide adsorbent, the present invention provides a method for preparing an organic oxide adsorbent, wherein a seed crystal is prepared by controlling a pH value and a two-stage crystallization process, and then a 13X molecular sieve with a high silicon-to-aluminum ratio, excellent specific surface area and pore capacity is prepared by aging treatment and hydrothermal crystallization treatment, wherein the prepared 13X molecular sieve has a high silicon source utilization rate and can provide more adsorption sites; then the surface and structure of the 13X molecular sieve are further modified to obtain an organic oxide adsorbent with a high silicon-to-aluminum ratio, high specific surface area and high pore capacity, wherein the surface and structure modification comprises introducing organic silicon into the 13X molecular sieve by reacting with an organic silicon coupling agent and calcining treatment to improve the dispersibility and stability of the adsorbent, increasing the adsorption sites by impregnation treatment with a copper salt solution, impregnation treatment with a titanium precursor and secondary calcination treatment, improving the adsorption capacity and selectivity of the adsorbent for organic oxides, and obtaining an adsorbent with excellent adsorption performance for organic oxides. The adsorbent prepared by the method of the present invention has a high silicon-to-aluminum ratio, a high specific surface area and a high pore capacity, and has excellent adsorption performance for organic oxides, and can achieve high-efficiency adsorption and removal of organic oxides in Fischer-Tropsch synthesis alkane-olefin products, hydrocarbon fuels or organic oxides in chemical products.

[0048] In order to obtain an organic oxide adsorbent with a high silicon-to-aluminum ratio and a high specific surface area, in a preferred embodiment, the silicon source is selected from one or more of silica sol, ethyl orthosilicate, macroporous silica gel, silicon powder, fly ash, and white carbon black, and the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate, and aluminum nitrate. The weight ratio of the silicon source to the aluminum source is (0.01-1.25):1; in order for the two to fully react and generate an organic oxide adsorbent with a high silicon-to-aluminum ratio and a high specific surface area, it is preferred that in step S1, the silicon-containing material The mass fraction of the silicon source in the material is 2% to 50%; preferably in step S1, the silicon source and water are stirred at 20 to 60°C for 0.1 to 12 hours to obtain an aluminum-containing material; preferably in step S1, the mass fraction of the aluminum source in the aluminum-containing material is 15% to 60%; preferably in step S1, the aluminum source and water are stirred at 20 to 60°C for 0.1 to 12 hours to obtain an aluminum-containing material; preferably in step S1, the stirring temperature is 20 to 100°C, and the stirring is carried out for 0.1 to 24 hours to obtain a first gel-like mother liquor.

[0049] In a preferred embodiment, the pH value of the first gel-like mother liquor is 11.8-12.5, which is conducive to the reaction of the silicon source and the aluminum source and further generates crystal seeds with high crystallinity, stable crystal form and structure in the two-stage thermal crystallization treatment, so as to further generate 13X molecular sieve with high silicon-to-aluminum ratio, specific surface area and pore capacity; in the preferred step S1, the pH value of the first gel-like mother liquor is adjusted by adding solid sodium hydroxide or by adding an aqueous solution of sodium hydroxide.

[0050] In a preferred embodiment, the crystallization temperature in the second stage of crystallization treatment is higher than the crystallization temperature in the first stage of crystallization treatment by more than 40°C, preferably, 50-60°C, and a two-stage hydrothermal crystallization treatment is adopted, wherein the 13X molecular sieve seeds with a high silicon-aluminum ratio generated in the first stage of crystallization treatment are further grown and optimized in the first stage of crystallization treatment to form a solution of 13X molecular sieve seeds with a complete structure, uniformity and high specific surface area. The use of the above-mentioned higher temperature difference is conducive to optimizing the adsorption of organic oxides with higher specific surface area; preferably, in the first stage of hydrothermal crystallization treatment, the crystallization temperature is 40-60°C, and the crystallization time is The time is 4 to 24 hours, more preferably 11 to 24 hours; preferably in the second hydrothermal crystallization treatment, the crystallization temperature is 90 to 100°C, and the crystallization time is 6 to 48 hours, more preferably 18 to 48 hours; preferably, the molar ratio of each component in the solution containing 13X molecular sieve seeds is: SiO2 / Al2O3=(0.01 to 6):1, Na2O / SiO2=(0.01 to 4.0):1, H2O / SiO2=(1.0 to 50.0):1, which is conducive to the subsequent growth of 13X molecular sieve with high adsorption performance; preferably, both stages of hydrothermal crystallization treatment are carried out in a hydrothermal reactor.

[0051] In order to obtain a 13X molecular sieve with a more regular and uniform structure, in a preferred embodiment, in step S2, the aging treatment is carried out under stirring conditions, the aging treatment temperature is 20-100°C, and the aging treatment time is 0.1-24h; in the preferred step S2, the hydrothermal crystallization treatment time is 0.1-36h; in the preferred step S2, the hydrothermal crystallization product is filtered and washed to neutrality, and then dried at 80-120°C to constant weight to obtain a 13X molecular sieve.

[0052] In order to obtain higher coupling efficiency and coupling effect, in a preferred embodiment, in step S3, the organosilicon coupling agent is selected from one or more of methyltriethoxysilane, isopropyltrimethoxysilane, vinyltrimethoxysilane, ethyl orthosilicate, ethoxysilane, ethyl orthosilicate, and 3-aminopropyltriethoxysilane, and the organic alcohol solvent is selected from one or more of ethanol, propanol, and butanol; in the preferred step S3, the mass ratio of 13X molecular sieve, organosilicon coupling agent and organic alcohol solvent is 1: (0.002-0.05): (0.8-2); in the preferred step S3, the reaction temperature is 15-40°C, and the reaction time is 1-10h; in the preferred step S3, the time of the first calcination treatment is 0.5-4h.

[0053] In a preferred embodiment, in step S3, the copper salt is selected from one or more of copper nitrate, copper chloride, and copper acetate; preferably in step S3, the concentration of the copper salt is 0.1 to 2 mol / L, and the soaking treatment time is 6 to 48 hours, thereby obtaining a higher adsorption capacity and selectivity of organic oxides while improving the utilization rate of the copper salt raw material.

[0054] In a preferred embodiment, in step S3, the titanium source in the titanium precursor sol is selected from one or more of tetrabutyl titanate, titanium orthosilicate or diisopropoxy diacetylacetonate titanium; preferably in step S3, the titanium precursor sol is formed by mixing a titanium source, ethanol and water, and ethanol and water are used as solvents to form a uniform titanium precursor sol, and the solvent is green and environmentally friendly; more preferably in step S3, the titanium source, ethanol and water are stirred and mixed at 50-70°C for 1-6h to form a titanium precursor sol; more preferably in step S3, ethanol and water are first mixed to form a mixed solvent, and then the titanium source is added for mixing; more preferably in step S3, the titanium source, ethanol and water are mixed in a mass ratio of 1:(3-7):(0.5-1.5); preferably in step S3, the drying temperature is 90-110°C, and the drying time is 6-18h; preferably in step S3, the second calcination time is 0.5-4h.

[0055] According to another aspect of the present invention, an organic oxide adsorbent is provided, which is prepared according to the above method for preparing an organic oxide adsorbent. The prepared organic oxide adsorbent has excellent specific surface area and pore capacity, which helps to improve the performance of the adsorbent in various applications, such as gas separation, pollutant removal, catalysis and other fields.

[0056] According to another aspect of the present invention, there is provided the use of the above organic oxide adsorbent in removing organic oxides from hydrocarbons; preferably, the hydrocarbons are hydrocarbon products produced by Fischer-Tropsch synthesis of coal, or olefin products produced by petroleum cracking; preferably, the organic oxides are selected from one or more of alcohols, aldehydes, ketones, and carboxylic acids having 1 to 21 carbon atoms, and the obtained organic oxide adsorbent has high adsorption capacity and selectivity for the organic oxides therein, especially for organic oxides in hydrocarbon products of various carbon numbers produced by Fischer-Tropsch synthesis or olefin products of various carbon numbers produced by petroleum cracking, especially C1 to C15 organic oxides, and has high adsorption efficiency, high capacity and high selectivity.

[0057] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0058] Example 1

[0059] A method for preparing an organic oxide adsorbent, the specific steps are as follows:

[0060] Step 1: dissolving 21.0 g of silica sol (mass fraction of silica is 30%) in 36.0 g of deionized water, and pre-treating in a closed reactor at 25° C. and 500 rpm for 1 hour to obtain a silicon-containing material;

[0061] Dissolve 24 g of aluminum sulfate in 18.0 g of deionized water, and stir at 25° C. and 500 rpm for 1 h to obtain an aluminum-containing material;

[0062] The aluminum-containing material liquid was added dropwise to the silicon-containing material, and stirring was continued at 60° C. for 8 h to obtain a gel solution;

[0063] 6.74 g of sodium hydroxide was dissolved in 36 g of an aqueous solution of sodium hydroxide prepared by deionization, and the solution was added to the gel solution until the pH value was 12 to obtain a gel solution;

[0064] The gel solution was placed in a hydrothermal reactor and subjected to two stages of hydrothermal crystallization treatment. In the first stage of the hydrothermal crystallization treatment, the crystallization temperature was 40°C and the crystallization time was 12 hours. In the second stage of the hydrothermal crystallization treatment, the crystallization temperature was 95°C and the crystallization time was 24 hours. A solution containing 13X molecular sieve seeds was obtained, wherein the molar ratio of each component in the solution containing 13X molecular sieve seeds was: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1.

[0065] Step 2: age the solution containing 13X molecular sieve seed crystals at 60°C for 12 hours, then perform hydrothermal crystallization at 80°C for 12 hours, filter the hydrothermal crystallization product, wash to neutrality, and dry to constant weight at 100°C to obtain 13X molecular sieve.

[0066] Step 3, add 50g of carbon-modified 13X molecular sieve and 0.5g of methyltriethoxysilane to 49.5g of anhydrous ethanol, stir and react at room temperature for 4 hours, then filter, and calcine the filtered molecular sieve at 450°C for 2 hours;

[0067] The calcined 13X molecular sieve was immersed in a 1 mol / L copper nitrate aqueous solution at room temperature for 24 hours;

[0068] 10 g of tetrabutyl titanate was added dropwise to a mixed solvent of 50 g of ethanol and 10 g of distilled water, and stirred at 60° C. for 3 hours to obtain a titanium precursor sol;

[0069] The 13X molecular sieve soaked in the copper salt solution is added to the titanium precursor sol, and after being stirred evenly, the mixture is dried at 100°C for 12 hours, and then heated to 500°C in a kiln at a heating rate of 5°C / min, and calcined for 2 hours;

[0070] The calcined product was dried by vacuum drying equipment for 12 hours to obtain a molecular sieve organic oxide adsorbent.

[0071] Example 2

[0072] Step 1: dissolving 1 g of silicon powder in 18 g of deionized water, and pre-treating in a closed reactor at 25° C. and 500 rpm for 1 hour to obtain a silicon-containing material;

[0073] 12 g of aluminum nitrate was dissolved in 18.0 g of deionized water, and stirred at 35° C. and 500 rpm for 1 hour to prepare an aluminum-containing material;

[0074] The aluminum-containing material was added dropwise to the silicon-containing material, and stirring was continued at 50° C. for 6 hours to obtain a gel solution;

[0075] An aqueous solution of sodium hydroxide prepared by dissolving 2 g of sodium hydroxide in 36 g of deionized water was added to the gel solution until the pH value was 11.8, thereby obtaining a gel solution;

[0076] The gel solution was transferred to a hydrothermal reactor and subjected to two hydrothermal crystallization treatments. In the first hydrothermal crystallization treatment, the crystallization temperature was 50°C and the crystallization time was 14 hours. In the second hydrothermal crystallization treatment, the crystallization temperature was 100°C and the crystallization time was 18 hours to obtain a solution containing 13X molecular sieve seeds. In the solution containing 13X molecular sieve seeds, the molar ratios of the components were: SiO2 / Al2O3=0.6:1, Na2O / SiO2=3:1, and H2O / SiO2=20:1.

[0077] Step 2: age the solution containing 13X molecular sieve seed crystals at 20°C for 0.1h, then perform hydrothermal crystallization at 60°C for 0.1h, filter the hydrothermal crystallization product, wash to neutrality, and dry at 80°C to constant weight to obtain 13X molecular sieve.

[0078] Step 3: add 50 g of carbon-modified 13X molecular sieve and 0.1 g of isopropyltrimethoxysilane to 40 g of anhydrous ethanol, stir and react at 15° C. for 1 hour, then filter, and calcine the filtered molecular sieve at 400° C. for 0.5 hour;

[0079] The calcined 13X molecular sieve was immersed in a 0.1 mol / L copper chloride aqueous solution at room temperature for 24 hours;

[0080] 10 g of titanium orthosilicate was added dropwise to a mixed solvent of 30 g of ethanol and 5 g of distilled water, and stirred at 50° C. for 1 hour to obtain a titanium precursor sol;

[0081] The 13X molecular sieve soaked in the copper salt solution was added to the titanium precursor sol, and after being stirred evenly, the mixture was dried at 90°C for 6 hours, and then heated to 450°C in a kiln at a heating rate of 5°C / min, and calcined for 0.5 hours;

[0082] Example 3

[0083] A method for preparing an organic oxide adsorbent, the specific steps are as follows:

[0084] Step 1: dissolving 0.17 g of silicon powder in 6 g of deionized water, and pre-treating in a closed reactor at 25° C. and 200 rpm for 1 hour to obtain a silicon-containing material;

[0085] 12 g of aluminum nitrate was dissolved in 18.0 g of deionized water, and stirred at 35° C. and 200 rpm for 1 hour to prepare an aluminum-containing material;

[0086] adding the aluminum source solution to the silicon-containing material and stirring at 100° C. for 24 hours to obtain a gel solution;

[0087] An aqueous solution of sodium hydroxide prepared by dissolving 0.9 g of sodium hydroxide in 6 g of deionized water was added to the gel solution until the pH value was 12.5. The prepared gel was then poured into a hydrothermal reactor for two-stage crystallization. First, crystallization was continued at 60° C. for 24 hours. Then, the temperature was increased to 120° C. for crystallization reaction for 48 hours to obtain a solution containing 13X molecular sieve seeds. The molar ratio of each component in the solution containing 13X molecular sieve seeds was: SiO2 / Al2O3=0.1:1, Na2O / SiO2=4:1, H2O / SiO2=1:1.

[0088] Step 2: age the solution containing 13X molecular sieve seed crystals at 100°C for 24 hours, then perform hydrothermal crystallization at 105°C for 36 hours, filter the hydrothermal crystallization product, wash to neutrality, and dry to constant weight at 120°C to obtain 13X molecular sieve.

[0089] (3) adding 50 g of carbon-modified 13X molecular sieve and 2.5 g of tetraethyl orthosilicate to 100 g of anhydrous ethanol, stirring and reacting at 40° C. for 10 hours, then filtering, and calcining the filtered molecular sieve at 500° C. for 4 hours;

[0090] The calcined 13X molecular sieve was immersed in a 2 mol / L copper acetate aqueous solution at room temperature for 24 hours;

[0091] 10 g of diisopropoxy diacetylacetonate titanium was added dropwise to a mixed solvent of 70 g of ethanol and 15 g of distilled water, and stirred at 70° C. for 6 hours to obtain a titanium precursor sol;

[0092] The 13X molecular sieve soaked in the copper salt solution was added to the titanium precursor sol, and after being stirred evenly, the mixture was dried at 110°C for 18 hours, and then heated to 550°C in a kiln at a heating rate of 5°C / min, and calcined for 4 hours;

[0093] The calcined product was dried by vacuum drying equipment for 12 hours to obtain an organic oxide adsorbent.

[0094] Example 4

[0095] The difference between the embodiment 1 and the embodiment 1 is that the step 1 is different. Specifically, the step 1 is as follows:

[0096] 14.65 g of ethyl orthosilicate was mixed with 36 g of deionized water, and pretreated in a closed reactor at 25° C. and 800 rpm for 1 hour to obtain a silicon-containing material;

[0097] Dissolve 12 g of aluminum nitrate in 18.0 g of deionized water, and stir at 35° C. and 800 rpm for 1 hour to obtain an aluminum-containing material;

[0098] The aluminum-containing material is gradually added dropwise to the silicon-containing material, and the mixture is mixed and stirred at 20° C. for 0.1 hour to prepare a gel solution;

[0099] 0.56 g of sodium hydroxide was dissolved in 6 g of deionized water to prepare a sodium hydroxide aqueous solution, which was poured into the gel solution until the pH value reached 8.5. The prepared gel was introduced into a hydrothermal reactor to perform a segmented crystallization reaction: first, the crystallization temperature was set to 20° C. for 4 hours; then it was increased to 80° C. and crystallization was maintained for 6 hours to obtain a solution containing 13X molecular sieve seeds, wherein the molar ratio of each component in the solution containing 13X molecular sieve seeds was: SiO2 / Al2O3=2.5:1, Na2O / SiO2=0.1:1, H2O / SiO2=40:1.

[0100] Example 5

[0101] The difference between the embodiment 1 and the embodiment 1 is that the methyltriethoxysilane in step (3) is replaced by 3-aminopropyltriethoxysilane.

[0102] Example 6

[0103] The only difference from Example 1 is that in the second stage of hydrothermal crystallization treatment, the crystallization temperature is 70°C.

[0104] Example 7

[0105] The only difference from Example 1 is that in the second stage of hydrothermal crystallization treatment, the crystallization temperature is 120°C.

[0106] Example 8

[0107] The only difference between this method and Example 1 is that the pH value of the gel solution is adjusted to 8.5 in step (1).

[0108] Comparative Example 1

[0109] The only difference between the embodiment 1 and the embodiment 1 is that the first hydrothermal crystallization treatment is performed in step 1. Specifically, step 1 is as follows:

[0110] Step 1: dissolving 21.0 g of silica sol (mass fraction of silica is 30%) in 36.0 g of deionized water, and pre-treating in a closed reactor at 25° C. and 500 rpm for 1 hour to obtain a silicon-containing material;

[0111] Dissolve 24 g of aluminum sulfate in 18.0 g of deionized water, and stir at 25° C. and 500 rpm for 1 h to obtain an aluminum-containing material;

[0112] The aluminum-containing material liquid was added dropwise to the silicon-containing material, and stirring was continued at 60° C. for 8 h to obtain a gel solution;

[0113] 6.74 g of sodium hydroxide was dissolved in 36 g of an aqueous solution of sodium hydroxide prepared by deionization, and the solution was added to the gel solution until the pH value was 12 to obtain a gel solution;

[0114] The gel solution was placed in a hydrothermal reactor for hydrothermal crystallization treatment at a crystallization temperature of 40° C. for 12 hours to obtain a solution containing 13X molecular sieve seed crystals.

[0115] Comparative Example 2

[0116] The only difference between the embodiment 1 and the embodiment 1 is that the second hydrothermal crystallization treatment is performed in step 1. Specifically, step 1 is as follows:

[0117] Step 1: dissolving 21.0 g of silica sol (mass fraction of silica is 30%) in 36.0 g of deionized water, and pre-treating in a closed reactor at 25° C. and 500 rpm for 1 hour to obtain a silicon-containing material;

[0118] Dissolve 24 g of aluminum sulfate in 18.0 g of deionized water, and stir at 25° C. and 500 rpm for 1 h to obtain an aluminum-containing material;

[0119] The aluminum-containing material liquid was added dropwise to the silicon-containing material, and stirring was continued at 60° C. for 8 h to obtain a gel solution;

[0120] 6.74 g of sodium hydroxide was dissolved in 36 g of an aqueous solution of sodium hydroxide prepared by deionization, and the solution was added to the gel solution until the pH value was 12 to obtain a gel solution;

[0121] The gel solution was placed in a hydrothermal reactor for hydrothermal crystallization treatment at a crystallization temperature of 95° C. for 24 hours to obtain a solution containing 13X molecular sieve seed crystals.

[0122] Comparative Example 3

[0123] The only difference from Example 1 is that step 3 is not performed. The specific steps are as follows:

[0124] Step 1: dissolving 21.0 g of silica sol (mass fraction of silica is 30%) in 36.0 g of deionized water, and pre-treating in a closed reactor at 25° C. and 500 rpm for 1 hour to obtain a silicon-containing material;

[0125] Dissolve 24 g of aluminum sulfate in 18.0 g of deionized water, and stir at 25° C. and 500 rpm for 1 h to obtain an aluminum-containing material;

[0126] The aluminum-containing material liquid was added dropwise to the silicon-containing material, and stirring was continued at 60° C. for 8 h to obtain a gel solution;

[0127] 6.74 g of sodium hydroxide was dissolved in 36 g of an aqueous solution of sodium hydroxide prepared by deionization, and the solution was added to the gel solution until the pH value was 12 to obtain a gel solution;

[0128] The gel solution was placed in a hydrothermal reactor and subjected to two stages of hydrothermal crystallization treatment. In the first stage of the hydrothermal crystallization treatment, the crystallization temperature was 40°C and the crystallization time was 12 hours. In the second stage of the hydrothermal crystallization treatment, the crystallization temperature was 95°C and the crystallization time was 24 hours. A solution containing 13X molecular sieve seeds was obtained, wherein the molar ratio of each component in the solution containing 13X molecular sieve seeds was: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1.

[0129] Step 2: age the solution containing 13X molecular sieve seed crystals at 60°C for 12 hours, then perform hydrothermal crystallization at 80°C for 12 hours, filter the hydrothermal crystallization product, wash to neutrality, and dry to constant weight at 100°C to obtain 13X molecular sieve.

[0130] Comparative Example 4

[0131] The only difference between the embodiment 1 and the embodiment 1 is that the copper salt solution immersion treatment is not performed in step 3. The specific steps are as follows:

[0132] Step 1: dissolving 21.0 g of silica sol (mass fraction of silica is 30%) in 36.0 g of deionized water, and pre-treating in a closed reactor at 25° C. and 500 rpm for 1 hour to obtain a silicon-containing material;

[0133] Dissolve 24 g of aluminum sulfate in 18.0 g of deionized water, and stir at 25° C. and 500 rpm for 1 h to obtain an aluminum-containing material;

[0134] The aluminum-containing material liquid was added dropwise to the silicon-containing material, and stirring was continued at 60° C. for 8 h to obtain a gel solution;

[0135] 6.74 g of sodium hydroxide was dissolved in 36 g of an aqueous solution of sodium hydroxide prepared by deionization, and the solution was added to the gel solution until the pH value was 12 to obtain a gel solution;

[0136] The gel solution was placed in a hydrothermal reactor and subjected to two stages of hydrothermal crystallization treatment. In the first stage of the hydrothermal crystallization treatment, the crystallization temperature was 40°C and the crystallization time was 12 hours. In the second stage of the hydrothermal crystallization treatment, the crystallization temperature was 95°C and the crystallization time was 24 hours. A solution containing 13X molecular sieve seeds was obtained, wherein the molar ratio of each component in the solution containing 13X molecular sieve seeds was: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1.

[0137] Step 2: age the solution containing 13X molecular sieve seed crystals at 60°C for 12 hours, then perform hydrothermal crystallization at 80°C for 12 hours, filter the hydrothermal crystallization product, wash to neutrality, and dry to constant weight at 100°C to obtain 13X molecular sieve.

[0138] Step 3, add 50g of carbon-modified 13X molecular sieve and 0.5g of methyltriethoxysilane to 49.5g of anhydrous ethanol, stir and react at room temperature for 4 hours, then filter, and calcine the filtered molecular sieve at 450°C for 2 hours;

[0139] 10 g of tetrabutyl titanate was added dropwise to a mixed solvent of 50 g of ethanol and 10 g of distilled water, and stirred at 60° C. for 3 hours to obtain a titanium precursor sol;

[0140] The calcined 13X molecular sieve was added to the titanium precursor sol, and after being stirred evenly, the mixture was dried at 100°C for 12 hours, and then heated to 500°C in a kiln at a heating rate of 5°C / min and calcined for 2 hours;

[0141] The calcined product was dried by vacuum drying equipment for 12 hours to obtain a molecular sieve organic oxide adsorbent.

[0142] Comparative Example 5

[0143] The only difference between the embodiment 1 and the embodiment 1 is that the titanium precursor sol treatment is not performed in step 3. The specific steps are as follows:

[0144] Step 1: dissolving 21.0 g of silica sol (mass fraction of silica is 30%) in 36.0 g of deionized water, and pre-treating in a closed reactor at 25° C. and 500 rpm for 1 hour to obtain a silicon-containing material;

[0145] Dissolve 24 g of aluminum sulfate in 18.0 g of deionized water, and stir at 25° C. and 500 rpm for 1 h to obtain an aluminum-containing material;

[0146] The aluminum-containing material liquid was added dropwise to the silicon-containing material, and stirring was continued at 60° C. for 8 h to obtain a gel solution;

[0147] 6.74 g of sodium hydroxide was dissolved in 36 g of an aqueous solution of sodium hydroxide prepared by deionization, and the solution was added to the gel solution until the pH value was 12 to obtain a gel solution;

[0148] The gel solution was placed in a hydrothermal reactor and subjected to two stages of hydrothermal crystallization treatment. In the first stage of the hydrothermal crystallization treatment, the crystallization temperature was 40°C and the crystallization time was 12 hours. In the second stage of the hydrothermal crystallization treatment, the crystallization temperature was 95°C and the crystallization time was 24 hours. A solution containing 13X molecular sieve seeds was obtained, wherein the molar ratio of each component in the solution containing 13X molecular sieve seeds was: SiO2 / Al2O3=1.5:1, Na2O / SiO2=1.6:1, H2O / SiO2=32:1.

[0149] Step 2: age the solution containing 13X molecular sieve seed crystals at 60°C for 12 hours, then perform hydrothermal crystallization at 80°C for 12 hours, filter the hydrothermal crystallization product, wash to neutrality, and dry to constant weight at 100°C to obtain 13X molecular sieve.

[0150] Step 3, add 50g of carbon-modified 13X molecular sieve and 0.5g of methyltriethoxysilane to 49.5g of anhydrous ethanol, stir and react at room temperature for 4 hours, then filter, and calcine the filtered molecular sieve at 450°C for 2 hours;

[0151] The calcined 13X molecular sieve was immersed in a 1 mol / L copper nitrate aqueous solution at room temperature for 24 hours;

[0152] The 13X molecular sieve soaked in the copper salt solution was dried at 100°C for 12 hours, and then heated to 500°C in a kiln at a heating rate of 5°C / min and calcined for 2 hours;

[0153] The calcined product was dried by vacuum drying equipment for 12 hours to obtain a molecular sieve organic oxide adsorbent.

[0154] 1. The silicon-aluminum ratio and specific surface area of ​​the organic oxide adsorbents prepared in the examples and comparative examples were tested respectively, and the results are shown in Table 1.

[0155] 2. The adsorption performance of the organic oxide adsorbent prepared in the embodiment and the comparative example was tested. The specific steps are as follows: taking the Fischer-Tropsch synthesis product as the adsorption object, passing it through a fixed bed containing the adsorbent, and monitoring the changes in product concentration before and after passing through the bed and the concentration changes of organic oxide impurities, and calculating the removal rate of organic oxygen compound impurities and the product loss rate, wherein the adsorption temperature is 55°C, the pressure is 1atm, the weight ratio of the adsorbent to the Fischer-Tropsch synthesis product is 1:10, the adsorbent loading is 1g, the sample enters the fixed bed reactor at a flow rate of 10ml / min, the adsorption time is 2 hours, and the content of each component in the Fischer-Tropsch synthesis product before treatment (in weight percentage) is shown in Table 2.

[0156] Table 1

[0157]

[0158]

[0159] Table 2

[0160]

[0161] As shown in Table 1, Examples 1 to 8 of the present invention prepared molecular sieve organic oxide adsorbents with high silicon-aluminum ratio, high specific surface area and high pore capacity. Specifically, the silicon-aluminum ratio was 2.2 to 2.9, and the pore volume was 0.39 cm 3 / g~0.5cm 3 / g, and the specific surface area is 800m 2 / g~910m 2 / g. Compared with Comparative Examples 1 and 2 using a single-stage crystallization process, Example 1 using two-stage crystallization significantly increases the specific surface area of ​​the adsorbent; from the data of Example 1 and Comparative Examples 3 to 5, it can be seen that the adsorption sites of organic oxides can be increased and product losses can be reduced through organosilicon modification treatment, copper salt solution impregnation treatment, titanium precursor sol impregnation treatment and secondary calcination treatment.

[0162] It can be seen from Table 2 that the molecular sieve organic oxide adsorbent prepared in Examples 1 to 8 has a good adsorption effect on the organic oxygen compounds in the different carbon number products of the Fischer-Tropsch synthesis, and almost does not adsorb the alkane products and olefin products of the Fischer-Tropsch synthesis, and has a high adsorption capacity and good selectivity for organic oxygen compounds.

[0163] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an organic oxide adsorbent, characterized in that: The steps include: Step S1, mixing a silicon source and water to obtain a silicon-containing material, mixing an aluminum source and water to obtain an aluminum-containing material, stirring and mixing the aluminum-containing material and the silicon-containing material to obtain a first gel-like mother liquor, adjusting the pH value of the first gel-like mother liquor to 8.5-12.5 using sodium hydroxide, and then performing two-stage hydrothermal crystallization treatment to obtain a solution containing 13X molecular sieve seed crystals; wherein the crystallization temperature of the first stage hydrothermal crystallization treatment is 20-60° C., and the crystallization temperature of the second stage hydrothermal crystallization treatment is 80-120° C.; Step S2, subjecting the solution containing the 13X molecular sieve seed crystals to an aging treatment, and then subjecting the solution to a hydrothermal crystallization treatment at 60-105° C., filtering, washing, and drying the hydrothermal crystallization product to obtain a 13X molecular sieve; Step S3, reacting the 13X molecular sieve and the organosilicon coupling agent in an organic alcohol solvent to obtain an organosilicon-modified 13X molecular sieve, soaking the product of the first calcination treatment in a copper salt solution to obtain a 13X molecular sieve impregnated with a copper salt solution, stirring and mixing the 13X molecular sieve impregnated with the copper salt solution and a titanium precursor sol to obtain a mixture, drying the mixture and then calcining it for a second time to obtain an organic oxide adsorbent; wherein the temperature of the first calcination treatment is 400-500°C, and the temperature of the second calcination treatment is 450-550°C.

2. The method for preparing an organic oxide adsorbent according to claim 1, characterized in that: The silicon source is selected from one or more of silica sol, tetraethyl orthosilicate, macroporous silica gel, silicon powder, fly ash, and white carbon black, and the aluminum source is selected from one or more of sodium aluminate, pseudo-boehmite, aluminum sulfate, and aluminum nitrate, and the weight ratio of the silicon source to the aluminum source is (0.01-1.25):1; Preferably, in step S1, the mass fraction of the silicon source in the silicon-containing material is 2% to 50%; Preferably, in the step S1, the silicon source and the water are stirred at 20 to 60° C. for 0.1 to 12 hours to obtain the silicon-containing material; Preferably, in step S1, the mass fraction of the aluminum source in the aluminum-containing material is 15% to 60%; Preferably, in the step S1, the aluminum source and the water are stirred at 20 to 60° C. for 0.1 to 12 hours to obtain the aluminum-containing material; Preferably, in the step S1, the mixture is stirred and mixed at a stirring temperature of 20 to 100° C. for 0.1 to 24 hours to obtain the first gel mother solution.

3. The method for preparing an organic oxide adsorbent according to claim 1 or 2, characterized in that: The pH value of the first gel-like mother solution is 11.8 to 12.5; Preferably, in step S1, the pH value of the first gel mother liquor is adjusted by adding solid sodium hydroxide or an aqueous solution of sodium hydroxide.

4. The method for preparing an organic oxide adsorbent according to any one of claims 1 to 3, characterized in that: The crystallization temperature in the second stage of crystallization treatment is higher than the crystallization temperature in the first stage of crystallization treatment by more than 40°C, preferably, by 50-60°C; Preferably, in the first hydrothermal crystallization treatment, the crystallization temperature is 40 to 60° C., and the crystallization time is 4 to 24 hours, more preferably 11 to 24 hours; Preferably, in the second hydrothermal crystallization treatment, the crystallization temperature is 90-100°C, and the crystallization time is 6-48h, more preferably 18-48h; Preferably, the molar ratio of each component in the solution containing 13X molecular sieve seeds is: SiO2 / Al2O3=(0.01-6):1, Na2O / SiO2=(0.01-4.0):1, H2O / SiO2=(1.0-50.0):

1.

5. The method for preparing an organic oxide adsorbent according to any one of claims 1 to 4, characterized in that: In the step S2, the aging treatment is carried out under stirring conditions, the temperature of the aging treatment is 20 to 100° C., and the time of the aging treatment is 0.1 to 24 hours; Preferably, in step S2, the hydrothermal crystallization treatment time is 0.1 to 36 hours; Preferably, in step S2, the hydrothermal crystallization product is filtered and washed to neutrality, and then dried at 80-120° C. to constant weight to obtain the 13X molecular sieve.

6. The method for preparing an organic oxide adsorbent according to any one of claims 1 to 5, characterized in that: In step S3, the organic silicon coupling agent is selected from one or more of methyltriethoxysilane, isopropyltrimethoxysilane, vinyltrimethoxysilane, ethyl orthosilicate, ethoxysilane, ethyl orthosilicate, and 3-aminopropyltriethoxysilane, and the organic alcohol solvent is selected from one or more of ethanol, propanol, and butanol; Preferably, in step S3, the mass ratio of the 13X molecular sieve, the organosilicon coupling agent and the organic alcohol solvent is 1: (0.002-0.05): (0.8-2); Preferably, in step S3, the reaction temperature is 15 to 40° C., and the reaction time is 1 to 10 h; Preferably, in step S3, the first calcination treatment is performed for 0.5 to 4 hours.

7. The method for preparing an organic oxide adsorbent according to any one of claims 1 to 6, characterized in that: In step S3, the copper salt is selected from one or more of copper nitrate, copper chloride, and copper acetate; Preferably, in step S3, the concentration of the copper salt is 0.1 to 2 mol / L, and the soaking treatment time is 6 to 48 hours.

8. The method for preparing an organic oxide adsorbent according to any one of claims 1 to 7, characterized in that: In the step S3, the titanium source in the titanium precursor sol is selected from one or more of tetrabutyl titanate, titanium orthosilicate or diisopropoxy diacetylacetonate titanium; Preferably, in step S3, the titanium precursor sol is formed by mixing a titanium source, ethanol and water; More preferably, in the step S3, the titanium source, the ethanol and the water are stirred and mixed at 50 to 70° C. for 1 to 6 hours to form the titanium precursor sol; More preferably, in step S3, the ethanol and the water are first mixed to form a mixed solvent, and then the titanium source is added to mix; More preferably, in step S3, the mass ratio of the titanium source, the ethanol and the water is 1:(3-7): (0.5~1.5) for mixing; Preferably, in step S3, the temperature of the drying process is 90 to 110° C., and the time of the drying process is 6 to 18 hours; Preferably, in step S3, the second calcination treatment is performed for 0.5 to 4 hours.

9. An organic oxide adsorbent, characterized in that: The organic oxide adsorbent is prepared according to the method for preparing the organic oxide adsorbent according to any one of claims 1 to 8.

10. Use of the organic oxide adsorbent according to claim 9 in removing organic oxides from hydrocarbons; Preferably, the hydrocarbon is a hydrocarbon product obtained by Fischer-Tropsch synthesis of coal, or an olefin product obtained by cracking petroleum; Preferably, the organic oxide is selected from one or more of alcohols, aldehydes, ketones and carboxylic acids having 1 to 21 carbon atoms.

Citation Information

Patent Citations

  • Method for removing heavy metal in traditional Chinese medicine by means of zeolite molecular sieve membrane

    CN105344130A

  • Preparation method silver-TiO2-nanometer copper oxide modified zeolite compound light catalyst

    CN106076398A

  • Preparation method for efficiently synthesizing 13X-type molecular sieve from calcined kaolin by microwave-assisted hydrothermal method

    CN108726533A

  • Interior surface modifications of molecular sieves with organometallic reagents and the use thereof for the conversion of oxygenates to olefins

    US20030187314A1

  • Method for manufacture of co-crystallized pentasil zeolite and zeolite mordenite in the presence of odso

    US20230330647A1