CuCe composite aerogel catalytic material as well as preparation method and application thereof

By loading copper oxide on the CeO2 airgel carrier and using copper and cerium doping to improve the redox capacity of the catalyst, the problem of efficient removal of CO and NO in automobile exhaust is solved and a high-depth purification effect is achieved.

CN118719074APending Publication Date: 2024-10-01INNER MONGOLIA UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410761139.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Pollutants (such as CO, NOx and particulate matter) in automobile exhaust pose a serious threat to the environment and human health, and existing technologies are difficult to effectively reduce their emissions.

Method used

Develop a CuCe composite aerogel catalytic material, using CeO2 aerogel as a carrier to support the transition metal oxide copper, and improving the redox capacity and oxygen storage capacity of the catalyst through copper and cerium doping to form a high specific surface area and high dispersion , a catalyst with high depth catalytic oxidation ability.

Benefits of technology

The catalyst significantly improves the conversion rate of CO and NO in the range of 200 to 600°C, enhances the purification ability of automobile exhaust, optimizes the active sites of the catalyst, prevents sintering deactivation, and improves catalytic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719074A_ABST
    Figure CN118719074A_ABST
Patent Text Reader

Abstract

The invention discloses a CuCe composite aerogel catalytic material and a preparation method and application thereof, belongs to the technical field of automobile exhaust catalysis, and provides the CuCe composite aerogel catalytic material and the preparation method and application thereof, by synthesizing a CeO2 aerogel carrier, the CeO2 aerogel carrier provides rich porosity, specific surface area and acid sites, and copper oxide is loaded, so that the catalytic performance of the CuCe composite aerogel catalytic material is improved. The CuCe composite oxide aerogel catalytic material with high specific surface area, high dispersity and high deep catalytic oxidation capacity is developed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of automobile exhaust catalysis, and in particular relates to a CuCe composite aerogel catalytic material and a preparation method and application thereof. Background Art

[0002] With the rapid development of social economy, the quality of life of the people is constantly improving, and the number of motor vehicles is growing rapidly. As the number of fuel-powered vehicles continues to increase, automobile exhaust emissions are increasing, which has brought catastrophic damage to the environment on which we depend for survival. There are four main types of pollutants in automobile exhaust: hydrocarbons, carbon monoxide, particulate matter, and nitrogen oxides. The emission of automobile exhaust pollutants mainly comes from fuel-powered vehicles. The emission of these pollutants can pose a great threat to people's health. For example, CO enters the human body and combines with hemoglobin, seriously endangering people's health. HC and NO x A reaction will occur to generate photochemical smog, which can cause serious harm to the human body and also lead to a large reduction in agricultural production. x It is easy to react with O2, and the reaction products can cause acid rain, which is harmful to organisms and buildings. Particulate matter (PM) is one of the main causes of haze.

[0003] In response to the above problems, in order to reduce the harm to people's health and the environment, relevant departments have studied and formulated relevant regulations. The emission standards for automobile exhaust have become more stringent. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a CuCe composite aerogel catalytic material and a preparation method and application thereof. By synthesizing a CeO2 aerogel carrier to provide rich porosity, specific surface area and acidic sites, copper oxide is loaded to develop a CuCe composite oxide aerogel catalytic material with high specific surface area, high dispersibility and high deep catalytic oxidation ability.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A CuCe composite aerogel catalytic material uses CeO2 aerogel as a carrier, and the carrier is loaded with transition metal oxide copper. According to different copper-cerium doping ratios, there is a strong synergistic effect between copper and cerium, which can improve the redox ability and oxygen storage capacity of the catalyst, and the introduction of copper can improve the redox performance of the cerium-based catalyst and form active oxygen species.

[0007] Furthermore, in the CeO2 aerogel, cerium nitrate is fixed at 0.02 mol, n(Ce):n(Cu)=1:(0.1-0.3), and different copper-cerium contents have an impact on the aerogel. The specific impact is: copper can promote the redox reaction of cerium and enhance the redox ability of the catalyst. The appropriate copper-cerium ratio can optimize the active sites of the catalyst, help maintain the structure and activity of the catalyst at high temperature, prevent sintering deactivation, and improve the catalytic efficiency.

[0008] Furthermore, the transition metal oxide is copper oxide (CuO).

[0009] The present invention also provides a method for preparing the CuCe composite aerogel catalytic material, comprising the following steps:

[0010] S1: dissolving Ce(NO3)3 in water to obtain a cerium salt aqueous solution, dropping the aqueous solution and an ammonia solution into water at room temperature, stirring, controlling the pH value to be alkaline, aging after the titration, filtering, and washing;

[0011] S2: The washed material in S1 is dried with supercritical carbon dioxide and naturally cooled to room temperature to obtain CeO2 aerogel;

[0012] S3: immersing the CeO2 aerogel in a copper salt solution, stirring, drying, and calcining to obtain the CuCe composite aerogel catalytic material.

[0013] Furthermore, in S1, the pH value is controlled to be 9±0.5; the titration is completed within 30 minutes; the aging time is 30 minutes; the washing is firstly washed with water and then washed with anhydrous ethanol. The present invention firstly washes with distilled water to remove nitrates in the gel, and then washes with anhydrous ethanol to remove water therein.

[0014] Furthermore, in S2, when supercritical carbon dioxide drying is performed, the pressure is 15 MPa, the temperature is 50°C, the pressure holding time is 4 hours, and the pressure release rate is 2 MPa / h.

[0015] Furthermore, in S3, the stirring time is 30 minutes; the drying temperature is 80°C; and the calcination is performed at 500°C for 4 hours.

[0016] The present invention also provides application of the CuCe composite aerogel catalytic material in automobile exhaust catalysts.

[0017] Furthermore, the CuCe composite aerogel catalytic material is used to catalyze CO and NO tail gases.

[0018] The catalyst prepared by this method uses cerium-based aerogel as a carrier, loads transition metal oxides, and uses the synergistic effect between copper and cerium and the high porosity and abundant acid sites of cerium aerogel to purify automobile exhaust. The special structure of cerium aerogel can provide abundant anchoring sites for active components, so that copper oxides are fully dispersed in the form of nanoparticles to form a highly composite oxide catalyst. The catalyst can oxidize CO to CO2 and reduce NO to N2 at a reaction temperature of 200-600°C.

[0019] Compared with the prior art, the present invention has the following advantages and technical effects:

[0020] The present invention uses CeO2 aerogel as a carrier to load copper oxide, and utilizes the high porosity and abundant acid sites of CeO2 aerogel to promote the rapid adsorption and decomposition of substrate molecules, so that copper oxide is completely dispersed in the form of nanoparticles to form a highly composite oxide catalyst. The active component CuO is directly highly composited with the CeO2 aerogel carrier, which improves the deep catalytic oxidation-reduction ability of the catalyst to automobile exhaust. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0022] Figure 1 This is a flow chart for preparing the CuCe composite aerogel catalytic material of the present invention;

[0023] Figure 2 is the conversion rate of CO of the CuCe composite aerogel catalytic material prepared in Examples 1-12;

[0024] Figure 3 The conversion rate of NO by the CuCe composite aerogel catalytic material prepared in Examples 1-12. DETAILED DESCRIPTION

[0025] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0026] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0027] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0028] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0029] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0030] Unless otherwise specified, the room temperature in the embodiments of the present invention is 25±2°C.

[0031] All raw materials used in the embodiments of the present invention are commercially available.

[0032] The technical solution of the present invention is further illustrated by the following embodiments.

[0033] Example 1

[0034] Take 9.304g (0.02mol) of Ce(NO3)3 and dissolve it in 30mL of deionized water. Stir thoroughly until dissolved to obtain a mixed solution. Add the above mixed solution and ammonia solution (concentration of 26%, the same below) dropwise into 400mL of distilled water at room temperature, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age for 30min and filter with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate therein, and then washed with anhydrous ethanol to remove the moisture therein and placed in a supercritical reactor for supercritical carbon dioxide drying at a pressure of 15MPa and a temperature of 50℃. The pressure is maintained for 4h and the pressure release rate is 2MPa / h. After naturally cooling to room temperature, the CeO2 aerogel is taken out. The prepared CeO2 aerogel was immersed in 1.45g copper nitrate solution (concentration of 50%, the same below) and stirred for 30min, dried at 80℃, and calcined at 400℃ for 4h to obtain a CuO / CeO2 composite aerogel catalyst, which is a CuCe composite aerogel catalytic material with a specific surface area of ​​463m 2 / g.

[0035] Example 2

[0036] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 1.45g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 500℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​377m 2 / g.

[0037] Example 3

[0038] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 1.45g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 600℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​303m 2 / g.

[0039] Example 4

[0040] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 0.966g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 400℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​361m 2 / g.

[0041] Example 5

[0042] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 0.966g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 500℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​266m 2 / g.

[0043] Example 6

[0044] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 0.966g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 600℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​227m 2 / g.

[0045] Example 7

[0046] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 0.483g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 400℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​479m 2 / g.

[0047] Example 8

[0048] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 0.483g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 500℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​422m 2 / g.

[0049] Example 9

[0050] Take 9.304g (0.02mol) of Ce (NO3) 3 and dissolve it in 30mL of deionized water, stir it thoroughly until it dissolves, and obtain a mixed solution. At room temperature, drop the mixed solution and ammonia solution into 400mL of distilled water, stir, control the pH value at 9±0.5, and control the titration speed so that the precipitation is completed in 30min. After the titration is completed, age it for 30min, and filter it with a vacuum pump. The obtained gel is washed with distilled water to remove the nitrate, and then washed with anhydrous ethanol to remove the water, and then placed in a supercritical reactor for supercritical carbon dioxide drying. The pressure is 15MPa, the temperature is 50℃, the pressure is maintained for 4h, the pressure release rate is 2MPa / h, and the aerogel is taken out after cooling naturally to room temperature. The prepared aerogel is immersed in 0.483g of copper nitrate solution and stirred for 30min, dried at 80℃, and calcined at 600℃ for 4h to obtain a CuCe composite aerogel catalytic material with a specific surface area of ​​351m 2 / g.

[0051] The conversion rates of CO and NO of the CuCe composite aerogel catalytic materials prepared in Examples 1-9 were tested. The specific testing method was as follows:

[0052] The present invention uses a fixed bed reaction device to carry out catalytic oxidation experiments of CO and NO on the prepared catalyst. The gas flow rate of the mixing box (Nanjing Boyuntong, GXDO8-4E) is 100 mL / min, and the air velocity is 8000 h -12000ppmCO, 500ppmNO (carbon-nitrogen ratio of 4:1) and 2% O2 were introduced into the gas mixing box to simulate automobile exhaust smoke, and the balance gas of the experiment of the present invention was N2. The temperature range of the experiment of the present invention was set to 200-600°C, a vertical tube furnace (Nanjing Boyuntong, VTL1600), and the heating rate of the tube furnace was 10°C / min.

[0053] Test results see Figure 2 and Figure 3 ,Depend on Figure 2 It can be seen that under the same conditions of the preparation method, as the reaction temperature continues to increase, the CO conversion rate of the catalyst gradually increases. From Examples 7-9, it can be seen that the catalyst with n(Ce):n(Cu)=1:0.1 has the best catalytic effect after being treated at 500°C, and the CO conversion rate can reach 72% at 200°C. When the temperature is increased to 300°C, the CO conversion rate reaches the highest, which is 91%. The CO conversion rate increases fastest at 200-300°C; from Examples 4-6, it can be seen that the catalyst with n(Ce):n(Cu)=1:0.2 has a CO conversion rate of 66% at 200°C, and when the temperature is increased to 400°C, the CO conversion rate reaches the highest, which is 90%. The CO conversion rate increases fastest at 200-300°C. It can be seen from Examples 1-3 that the CO conversion rate of the catalyst with n(Ce):n(Cu)=1:0.3 at 200°C is 42%. When the temperature is increased to 600°C, the CO conversion rate reaches the highest, which is 72%. The CO conversion rate increases fastest at 200-300°C.

[0054] Depend on Figure 3 It can be seen that: under the same preparation method, as the reaction temperature continues to increase, the NO conversion rate of the catalyst is a process from low to high. As can be seen from Examples 7-9, the catalyst with n(Ce):n(Cu)=1:0.1 has the best catalytic effect after treatment at 500°C, and the conversion rate of NO is 48% at 200°C. When the temperature is increased to 600°C, the conversion rate of NO reaches the highest, which is 91%, and the conversion rate of NO increases fastest at 300-500°C; As can be seen from Examples 4-6, the conversion rate of NO at 200°C for the catalyst with n(Ce):n(Cu)=1:0.2 is 43%, when the temperature is increased to 600°C, the conversion rate of NO reaches the highest, which is 88%, and the conversion rate of NO increases fastest at 300-500°C; As can be seen from Examples 1-3, the conversion rate of NO at 200°C for the catalyst with n(Ce):n(Cu)=1:0.3 is 32%, when the temperature is increased to 600°C, the conversion rate of NO reaches the highest, which is 86%, and the conversion rate of NO increases fastest at 300-500°C.

[0055] Comparative Example 1

[0056] Same as Example 1, except that the calcination temperature is 1200°C.

[0057] In this comparative example, the aerogel carrier is white and opaque after being calcined at 1200° C. Its density is calculated to be very low. After being calcined at 1200° C. for two hours, it will break into many small pieces. The linear shrinkage rate reaches about 60%, and the stability of the aerogel is reduced.

[0058] Comparative Example 2

[0059] Same as Example 1, except that copper oxide is not loaded.

[0060] In this comparative example, since no copper element is added, the copper species provides additional active sites on the catalyst surface, which is conducive to the adsorption and oxidation of CO. Without the presence of copper, the active sites are reduced and the catalytic activity is reduced. At the same time, the addition of copper is conducive to broadening the effective operating temperature window of the catalyst, especially improving the catalytic activity of the catalyst at low temperatures. Not loading copper may cause the performance of the catalyst to decrease within a certain temperature range.

[0061] Comparative Example 3

[0062] Same as Example 1, except that cerium is not added.

[0063] In this comparative example, since the cerium content is changed, the cerium-based material can store and release oxygen. The lack of cerium causes its oxygen storage capacity to weaken and changes the surface properties of the catalyst. Without cerium, the number of active sites of the catalyst may be reduced.

[0064] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A CuCe composite aerogel catalytic material, characterized in that: CeO2 aerogel is used as a carrier, and transition metal oxide is loaded on the carrier.

2. The CuCe composite aerogel catalytic material according to claim 1, characterized in that: The copper salt is copper nitrate trihydrate, and the cerium salt is cerium nitrate hexahydrate.

3. The CuCe composite aerogel catalytic material according to claim 1, characterized in that: n(Ce):n(Cu)=1:(0.1-0.3).

4. A method for preparing the CuCe composite aerogel catalytic material according to any one of claims 1 to 3, characterized in that: The steps include: S1: dissolving Ce(NO3)3 in water to obtain a cerium salt aqueous solution, dropping the aqueous solution and an ammonia solution into water at room temperature, stirring, controlling the pH value to be alkaline, aging after the titration, filtering, and washing; S2: The washed material in S1 is dried with supercritical carbon dioxide and naturally cooled to room temperature to obtain CeO2 aerogel; S3: immersing the CeO2 aerogel in a copper salt solution, stirring, drying, and calcining to obtain the CuCe composite aerogel catalytic material.

5. The method for preparing the CuCe composite aerogel catalytic material according to claim 4, characterized in that: In S1, the pH value is controlled to be 9±0.5; the titration is completed within 30 minutes; the aging time is 30 minutes; and the washing is firstly washed with water and then washed with anhydrous ethanol.

6. The method for preparing the CuCe composite aerogel catalytic material according to claim 4, characterized in that: In S2, when supercritical carbon dioxide drying is performed, the pressure is 15 MPa, the temperature is 50°C, the pressure holding time is 4 h, and the pressure release rate is 2 MPa / h.

7. The method for preparing the CuCe composite aerogel catalytic material according to claim 4, characterized in that: In S3, the stirring time is 30 minutes; the drying temperature is 80°C; and the calcination is performed at 500°C for 4 hours.

8. Use of the CuCe composite aerogel catalytic material according to any one of claims 1 to 3 in automobile exhaust catalysts.

9. Use of the CuCe composite aerogel catalytic material according to any one of claims 1 to 3 in catalyzing CO and NO tail gases.

Citation Information

Patent Citations

  • Aerogel catalyst as well as preparation method and application thereof