Methanol washing acid gas and methanol flash steam catalyst sulfuration method
By using methanol wash acid gas and methanol flash gas to replace the traditional carbon disulfide, and reacting with the catalyst after heating, the problems of high hydrogen consumption and safety hazards of carbon disulfide in the traditional vulcanization process are solved, and a low-cost and environmentally friendly catalyst vulcanization effect is achieved.
Patent Information
- Application Number
- CN202410881806.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
AI Technical Summary
During the sulfurization process of traditional Co-Mo catalysts, hydrogen consumption is high, and carbon disulfide is flammable and explosive, posing safety risks and wasting resources, resulting in high production costs and serious environmental pollution.
Methanol wash acid gas and methanol flash gas are used to replace carbon disulfide. After heating, it reacts with the catalyst through a conversion furnace to generate CoS and MoS2. A low-temperature sulfurization process and cyclic sulfurization are used to control the temperature and gas flow rate of the sulfide gas to reduce hydrogen consumption and carbon disulfide. use.
The consumption of hydrogen and carbon disulfide is reduced, the vulcanization efficiency is improved, production costs and environmental pollution are reduced, and the safety and economic benefits of the process are improved.
Smart Images

Figure CN118719098A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of methanol-washed acid gas and methanol flash gas catalyst sulfurization, in particular to a methanol-washed acid gas and methanol flash gas catalyst sulfurization method. Background Art
[0002] In coal chemical production, the catalyst commonly used in the conversion position is the Co-Mo series conversion catalyst. The molybdenum-cobalt catalyst has high catalytic activity, selectivity and high stability, and can maintain catalytic activity for a long time; it also has a large specific surface area and pore structure, which is conducive to the adsorption and diffusion of reactant molecules and improves the reaction rate. It is currently widely used in synthetic ammonia plants and has achieved significant energy-saving and consumption-reducing effects. The Co-Mo series conversion catalyst exists in the form of cobalt oxide and molybdenum oxide when it leaves the factory, and has no conversion activity. Before use, it needs to be sulfurized to convert the oxidized cobalt and molybdenum into a sulfurized state to show high conversion activity. The traditional sulfurization method is that semi-water gas at a certain temperature passes through a container filled with a sulfurizing agent to produce a sulfurized raw gas containing a certain concentration of hydrogen sulfide. The gas passes through the Co-Mo catalyst bed and gradually converts CoO and MoO3 in the catalyst into CoS and MoS2. The most commonly used hydrogenation cycle sulfurization method for the current Co-Mo series catalyst sulfurization is the following reaction:
[0003] MoO3+2H2S+H2=MoS2+3H2OΔH 0 =-48.2KJ / mo
[0004] CoO+H2S=CoS+H2OΔH 0 =-13.4KJ / mo
[0005] CS2+4H2=2H2S+CH4ΔH 0 =-240KJ / mo.
[0006] H2 consumption during the sulfidation process: Theoretically, 85Nm3 of hydrogen is required for the complete sulfidation of each ton of QDB. When cyclic sulfidation is adopted, the outlet of the conversion furnace should be kept at 15-20% of hydrogen. According to the sulfidation experience, the hydrogen consumption is about 3 times the theoretical amount, resulting in a waste of hydrogen resources. Moreover, during the sulfidation process, CS2 needs to be continuously added above 180°C to react with hydrogen to generate more H2S. CS2 is a colorless or light yellow transparent liquid with a pungent odor and is volatile. It has a melting point of -111.5°C and a boiling point of 46.3°C. It is a low flash point flammable liquid. Its vapor can form a wide range of explosive mixtures with air. Friction, heat, open flames or contact with oxidants can easily cause combustion and explosion. Moreover, carbon disulfide is a poison that damages the nervous system and vascular system. It is very unsafe and inconvenient in transportation, storage and use, and accidents such as fire and even explosion often occur.
[0007] In order to rationally utilize resources, reduce production costs, improve traditional sulfiding technology, and rationally utilize resources, after many investigations, analyses, demonstrations and experiments, we have explored a new sulfiding technology, namely: using pulverized coal gasification methanol to wash acid gas and methanol flash gas to replace the traditional carbon disulfide hydrogenation process sulfidation scheme, achieving good economic and social benefits.
[0008] Therefore, it is necessary to provide a method for methanol washing acid gas and methanol flash gas catalyst sulfidation to solve the above technical problems. Summary of the invention
[0009] The invention provides a method for sulfurizing a methanol-washed acid gas and a methanol flash gas catalyst, which solves the problems in the background technology.
[0010] In order to solve the above technical problems, the present invention provides a method for sulfurizing a methanol-washed acid gas and a methanol flash gas catalyst, comprising the following steps:
[0011] S1, through the Roots blower, the heat carrier N2 and CO2, the methanol washing acid gas for sulfidation, and the methanol flash gas are pressurized and heated in an electric furnace before entering the conversion furnace;
[0012] S2, providing a place for catalyst sulfidation through a conversion furnace, where methanol-washed acid gas, synthetic flash gas and catalyst react to sulfidate the catalyst;
[0013] S3, cooling and lowering the temperature of the sulfide gas by a cooler;
[0014] S4, separating the generated water through a deamination tower;
[0015] S5. The separated gas is pressurized by a Roots blower and then recycled for vulcanization.
[0016] Preferably, the specific method of sulfurization in the S2 is to use N2 and CO2 as carriers, methanol-washed acid gas and methanol flash gas as sulfurizing agents, and continuously add methanol-washed acid gas and methanol flash gas at above 200°C, so that H2 and H2S react with CoO and MoO3 to generate CoS and MOS2.
[0017] Preferably, the reaction chemical formula of the sulfurization in S2 is:
[0018] MoO3+2H2S+H2=MoS2+3H2OΔH 0 =-48.2KJ / mo
[0019] CoO+H2S=CoS+H2OΔH 0 =-13.4KJ / mo.
[0020] Preferably, the temperature rise vulcanization of the catalyst can be divided into five stages: displacement temperature rise, initial vulcanization period, main vulcanization period, final vulcanization period and temperature drop and sulfur removal period.
[0021] Preferably, the replacement heating stage: the sulfurization heating period is an important stage during the catalyst heating and sulfurization period, which mainly evaporates the physical moisture of the catalyst layer; first, the heating process is opened, and when the nitrogen pressure of the system is controlled at 30KPa, the heating fan is turned on, and the fan outlet pressure is controlled at about 60kPa. Depending on the nitrogen feeding amount and the system outlet venting amount, the system pressure is stabilized, the catalyst air velocity is controlled to 300-500h-1, and the heating rate is about 30℃ / h (the heating rate should not exceed 50℃ / h), and the temperature is increased according to the heating curve; when the bed temperature rises to 120℃, the temperature is kept constant for about 4h to release the physical water adsorbed in the catalyst. When the bed temperature rises to 200℃-220℃, the temperature is kept constant for about 4h to reduce the bed temperature difference, and the heating ends; add an appropriate amount of methanol flash gas, and when the hydrogen content at the bed outlet is analyzed to be 5-10%, the sulfurization heating can be turned on.
[0022] Preferably, in the initial stage of the sulfidation: when the inlet temperature of the conversion furnace is greater than 220°C and the temperature of the lowest point of the catalyst layer is not less than 200°C, the methanol-washed acid gas can be added, and the hydrogen sulfide concentration is 18-25% according to the sulfuric acid production process requirements; when the catalyst bed temperature of the conversion furnace is greater than 220°C, start to add methanol-washed acid gas to the fan inlet to sulfide the catalyst, observe the change of bed temperature rise, the heating rate is 10-15°C / h, the air velocity is 300-500h-1, and the acid gas replenishment amount is controlled to be stable at the inlet flow rate of 50-100m3 / h at the beginning; the amount of acid gas added in the initial stage of sulfidation is slowly increased from small to large; the temperature is adjusted mainly by the electric heater and supplemented by the gas volume; the hot spot temperature in the initial stage of sulfidation shall not exceed 280°C.
[0023] Preferably, the main sulfurization period: when the bed temperature reaches 260-300°C, when the outlet H2S is ≥3.0g / Nm3, and the hydrogen content is greater than 5%, the main sulfurization period can be entered, the acid gas feed rate at the fan inlet is increased to 100-200m3 / h, the catalyst is sulfurized, and the bed temperature is slowly raised to about 350°C and stabilized for 4 hours. If the outlet H2S is still around 10g / Nm3, the bed temperature should continue to be raised to about 400°C and kept constant for 4 hours. If it does not reach 400°C, it can be appropriately extended for 1-2 hours to allow H2S to penetrate the catalyst bed; when H2S penetrates the bed outlet, the acid gas feed rate can be increased to continue to sulfurize the catalyst, and the acid gas feed rate can be increased to 1500-2000m3 / h.
[0024] Preferably, at the end of the vulcanization, the hot spot temperature is maintained at 400-430°C, ensuring that the temperature at each point of the bed is maintained at 400-430°C for 4 hours. When the H2S at the outlet of the isothermal furnace is ≥15g / Nm3 and the hydrogen content is greater than 5%, the vulcanization is considered to be completed, the inlet and outlet valves and the vent valve are closed, and the furnace is stuffy for 4 hours.
[0025] Preferably, the cooling and sulfur removal period: after the sulfurization is completed, the power of the electric heater is gradually reduced, the amount of acid gas added is reduced to cool down, the amount of methanol flash gas added is closed, the venting and sulfur removal to the flare are opened, and when the temperature drops below 300°C, the acid gas is stopped, and the nitrogen gas volume is increased to continue to reduce the bed temperature to below 270°C. When the outlet H2S is analyzed to be <1.0g / Nm3, the cooling and sulfur removal is considered to be completed, and the cooling rate is <50°C / h.
[0026] Preferably, it also includes a monitoring system for monitoring the temperature of the sulfiding gas, which includes a data acquisition module, a central processing module, a data reference module, an editing module, a communication module, a temperature control module and a gas control module.
[0027] Compared with the related art, the methanol-washed acid gas and methanol flash gas catalyst sulfidation method provided by the present invention has the following beneficial effects:
[0028] The invention provides a method for sulfurizing a catalyst using methanol-washed acid gas and methanol flash gas. The invention adopts a conversion sulfurization process of low-temperature methanol-washed acid gas with hydrogen sulfide and methanol flash gas with hydrogen, which changes the traditional sulfurization process of carbon disulfide hydrogenation. Theoretically, 85Nm3 of hydrogen must be consumed for complete sulfurization of each ton of catalyst during the traditional hydrogenation cycle sulfurization. During sulfurization, the outlet of the conversion furnace must contain 15-20% of hydrogen. According to sulfurization experience, the hydrogen consumption is about 3 times the theoretical amount, and 80kg of CS2 is required for each ton of catalyst, which consumes a large amount of hydrogen resources and CS2, resulting in high production costs and serious environmental pollution. The conversion sulfurization process of methanol-washed acid gas with hydrogen sulfide and methanol flash gas with hydrogen overcomes the above-mentioned many unfavorable factors and achieves good economic benefits, environmental benefits and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A sulfurization flow chart of the first embodiment of the sulfurization method for methanol-washed acid gas and methanol flash gas catalyst provided by the present invention;
[0030] Figure 2 A temperature rise curve diagram of the methanol-washed acid gas and methanol flash gas catalyst sulfidation method provided by the present invention;
[0031] Figure 3 This is a structural schematic diagram of the first embodiment of the methanol-washed acid gas and methanol flash vapor catalyst sulfidation method provided by the present invention. DETAILED DESCRIPTION
[0032] The present invention will be further described below in conjunction with the accompanying drawings and implementation modes.
[0033] First embodiment
[0034] Please refer to Figure 1 , Figure 2 ,in, Figure 1 A sulfurization flow chart of the sulfurization method of methanol-washed acid gas and methanol flash gas catalyst provided by the present invention; Figure 2 The temperature rise curve of the methanol-washed acid gas and methanol flash vapor catalyst sulfidation method provided by the present invention. The methanol-washed acid gas and methanol flash vapor catalyst sulfidation method comprises the following steps:
[0035] S1, through the Roots blower, the heat carrier N2 and CO2, the methanol washing acid gas for sulfidation, and the methanol flash gas are pressurized and heated in an electric furnace before entering the conversion furnace;
[0036] S2, providing a place for catalyst sulfidation through a conversion furnace, where methanol-washed acid gas, synthetic flash gas and catalyst react to sulfidate the catalyst;
[0037] S3, cooling and lowering the temperature of the sulfide gas by a cooler;
[0038] S4, separating the generated water through a deamination tower;
[0039] S5. The separated gas is pressurized by a Roots blower and then recycled for vulcanization.
[0040] Feasibility analysis of methanol washing acid gas and methanol flash gas sulfidation:
[0041] During normal operation, methanol-washed acid gas and methanol flash gas are both recycled and reused as waste gas. Methanol-washed acid gas is sent to sulfur recovery treatment and sulfuric acid is produced as a by-product; flash gas is incinerated in the waste heat recovery system and steam is produced as a by-product, which is both environmentally friendly and resource-saving. Its gas composition is as follows:
[0042]
[0043] From the analysis of gas composition, it is obvious that methanol-washed acid gas and methanol flash gas contain sulfurized inert heat carrier gases CO2 and N2, as well as H2S and H2 that react with CoO and MoO3 to generate CoS and MOS2. By rationally allocating the gas amounts of methanol-washed acid gas and methanol flash gas, the sulfurization operation of the conversion device can be carried out.
[0044] The specific method of sulfurization in S2 is to use N2 and CO2 as carriers, methanol-washed acid gas and methanol flash vapor as sulfurizing agents, and continuously add methanol-washed acid gas and methanol flash vapor at above 200°C, so that H2 and H2S react with CoO and MoO3 to generate CoS and MOS2.
[0045] The reaction chemical formula of the sulfurization in S2 is:
[0046] MoO3+2H2S+H2=MoS2+3H2OΔH 0 =-48.2KJ / mo
[0047] CoO+H2S=CoS+H2OΔH 0 =-13.4KJ / mo.
[0048] During the vulcanization, methanol is used to wash the acid gas and methanol flash gas as the vulcanizing agent, and the vulcanization and strengthening are carried out in a cycle. During the vulcanization process, the system pressure is kept as low as possible to prevent steam and water from entering.
[0049] The process of heating and sulfiding gas is as follows:
[0050] The nitrogen from the aerospace furnace is pressurized by the Roots blower and then enters the system → adds methanol to wash the acid gas → electric furnace → adds methanol flash steam → conversion furnace → cooler → deamination tower → Roots blower inlet.
[0051] The process of heating sulfide water is: synthetic circulating water supply main pipe → cooler → discharge to synthetic circulating water return main pipe.
[0052] Preparation work before catalyst sulfidation:
[0053] 1) After the conversion catalyst is loaded, the conversion system is tested for airtightness;
[0054] 2) The nitrogen system is replaced and qualified, and the O2 of each leaching sampling analysis is ≤0.2%;
[0055] 3) The electric heater is debugged normally and can be used at any time;
[0056] 4) The heating fan test operation is normal;
[0057] 5) Instrument debugging is normal;
[0058] 6) Prepare the reports and temperature rise curve drawing tables required during the temperature rise vulcanization period.
[0059] The temperature rise vulcanization of the catalyst can be divided into five stages: displacement temperature rise, initial vulcanization period, main vulcanization period, final vulcanization period and temperature drop and sulfur discharge period.
[0060] The replacement heating stage: the vulcanization heating period is an important stage during the catalyst heating and vulcanization period, which mainly evaporates the physical moisture of the catalyst layer; first, the heating process is opened, and when the nitrogen pressure added to the system is controlled at 30KPa, the heating fan is turned on, and the fan outlet pressure is controlled at about 60kPa. Depending on the nitrogen supply amount and the system outlet venting amount, the system pressure is stabilized, the catalyst air velocity is controlled to 300-500h-1, and the heating rate is about 30℃ / h (the heating rate should not exceed 50℃ / h). According to the heating curve ( Figure 2 ) to increase the temperature; when the bed temperature rises to 120℃, keep the temperature constant for about 4 hours to release the physical water adsorbed in the catalyst. When the bed temperature rises to 200℃-220℃, keep the temperature constant for about 4 hours to reduce the bed temperature difference and end the heating; add an appropriate amount of methanol flash gas, and when the hydrogen content at the bed outlet is analyzed to be 5-10%, the sulfidation heating can be started.
[0061] In the initial stage of sulfidation: when the inlet temperature of the conversion furnace is greater than 220°C and the temperature of the lowest point of the catalyst layer is not less than 200°C, methanol-washed acid gas can be added, and the hydrogen sulfide concentration is 18-25% according to the requirements of the sulfuric acid production process; when the catalyst bed temperature of the conversion furnace is greater than 220°C, methanol-washed acid gas is added to the fan inlet to sulfide the catalyst, and the bed temperature rise changes are observed. The heating rate is 10-15°C / h, and the air velocity is 300-500h-1. At the beginning, the amount of acid gas added is controlled to be stable at the inlet flow rate of 50-100m3 / h; in the initial stage of sulfidation, the amount of acid gas added is slowly increased from small to large; the temperature is adjusted mainly by the electric heater and supplemented by adjusting the gas volume; the hot spot temperature in the initial stage of sulfidation shall not exceed 280°C.
[0062] The main sulfurization period: when the bed temperature reaches 260-300°C, when the outlet H2S is ≥3.0g / Nm3, and the hydrogen content is greater than 5%, the main sulfurization period can be entered, the acid gas supplement at the fan inlet is increased to 100-200m3 / h, the catalyst is sulfurized, and the bed temperature is slowly raised to about 350°C and stabilized for 4 hours. If the outlet H2S is still around 10g / Nm3, the bed temperature should continue to be raised to about 400°C and kept at a constant temperature for 4 hours. If it does not reach 400°C, it can be appropriately extended for 1-2 hours to allow H2S to penetrate the catalyst bed; when H2S penetrates the bed outlet, the acid gas supplement can be increased to continue to sulfurize the catalyst, and the acid gas supplement can be increased to 1500-2000m3 / h.
[0063] At the end of the vulcanization, the hot spot temperature is maintained at 400-430°C, ensuring that the temperature of each point in the bed is maintained at 400-430°C for 4 hours. When the H2S at the outlet of the conversion furnace is ≥15g / Nm3 and the hydrogen content is greater than 5%, the vulcanization is considered to be completed, the inlet and outlet valves and the vent valve are closed, and the furnace is stuffy for 4 hours.
[0064] The cooling and sulfur removal period: after the sulfurization is completed, gradually reduce the power of the electric heater, reduce the amount of acid gas added to cool down, close the amount of methanol flash gas, open the vent to discharge sulfur to the flare, when the temperature drops below 300°C, stop adding acid gas, increase the amount of nitrogen to continue to reduce the bed temperature to below 270°C, and when the outlet H2S is analyzed to be <1.0g / Nm3, the cooling and sulfur removal is considered to be completed, and the cooling rate is <50°C / h.
[0065] Reference scheme for temperature rise vulcanization in conversion furnace
[0066]
[0067] The working principle of the methanol-washed acid gas and methanol flash gas catalyst sulfurization method provided by the present invention is as follows:
[0068] A small amount of nitrogen from the aerospace furnace is pressurized by a Roots blower and then enters the system. Methanol is added to the acid gas washed at the inlet of the Roots blower and then enters the electric heater for heating. After heating, methanol flash gas is added and mixed. After mixing, the mixture enters the controllable heat transfer conversion reactor for sulfurization, and then enters the conversion gas cooler for cooling. Finally, the generated water is separated in the deamination tower, and the separated gas is pressurized by a Roots blower and then circulated for sulfurization.
[0069] Compared with the related art, the methanol-washed acid gas and methanol flash gas catalyst sulfidation method provided by the present invention has the following beneficial effects:
[0070] The present invention adopts a conversion sulfurization process of low-temperature methanol-washed acidic gas with hydrogen sulfide and methanol flash gas with hydrogen, which changes the traditional carbon disulfide hydrogenation sulfurization process. According to the traditional hydrogenation cycle sulfurization, 85Nm3 of hydrogen is required for complete sulfurization of each ton of catalyst in theory, and the hydrogen content at the outlet of the conversion furnace should be maintained at 15-20% during sulfurization. According to sulfurization experience, the hydrogen consumption is about 3 times the theoretical amount, and 80kg of CS2 is required for each ton of catalyst, which consumes a large amount of hydrogen resources and CS2, resulting in high production costs and serious environmental pollution. The conversion sulfurization process of methanol-washed acidic gas with hydrogen sulfide and methanol flash gas with hydrogen overcomes the above-mentioned many unfavorable factors and achieves good economic benefits, environmental benefits and social benefits.
[0071] Second embodiment
[0072] Please refer to Figure 3 Based on the methanol-washed acid gas and methanol flash vapor catalyst sulfidation method provided in the first embodiment of the present application, the second embodiment of the present application proposes another methanol-washed acid gas and methanol flash vapor catalyst sulfidation method. The second embodiment is only a preferred embodiment of the first embodiment, and the implementation of the second embodiment will not affect the independent implementation of the first embodiment.
[0073] Specifically, the difference between the methanol-washed acid gas and methanol flash gas catalyst sulfidation method provided in the second embodiment of the present application is that it also includes a monitoring system for monitoring the temperature of the sulfided gas, which includes a data acquisition module, a central processing module, a data reference module, an editing module, a communication module, a temperature control module and a gas control module.
[0074] The output end of the data acquisition module is connected to the input end of the central processing module, the input end of the data reference module is connected to the output end of the central processing module, the output end of the editing module is connected to the input end of the data reference module, the input end of the communication module is connected to the output end of the central processing module, the input end of the temperature control module is connected to the output end of the central processing module, and the input end of the gas control module is connected to the output end of the central processing module.
[0075] The temperature of the electric furnace, conversion furnace, cooler and deamination tower is collected through the data acquisition module, and the collected data is transmitted to the central processing module, which is aligned and analyzed and sorted, and then compared with the data through the data reference module. When the temperature does not meet the preset standard, the temperature is changed through the temperature control module to meet the preset standard. At the same time, the gas control module can control the amount of each gas introduced. The data reference module can preset the standard temperature value of each equipment in the process of methanol washing acid gas and methanol flash gas catalyst sulfidation. When the central processing module compares it with the standard temperature, it can be adjusted in time if it is found that the temperature does not meet the standard. The preset temperature value in the data reference module can be adjusted through the setting of the editing module. The setting of the communication module can transmit a signal to the staff for inspection when the unit is unstable and the preset temperature value is not reached.
[0076] Compared with the related art, the methanol-washed acid gas and methanol flash gas catalyst sulfidation method provided by the present invention has the following beneficial effects:
[0077] The present invention can monitor the temperature of the entire process, meet process requirements, avoid high or low temperature phenomena, and at the same time can control the amount of gas when the temperature reaches a preset value to ensure safe and stable operation of the unit.
[0078] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for sulfurizing a methanol-washed acid gas or methanol flash gas catalyst, characterized in that: The following steps are involved: S1, through the Roots blower, the heat carrier N2 and CO2, the methanol washing acid gas for sulfidation, and the methanol flash gas are pressurized and heated in an electric furnace before entering the conversion furnace; S2, providing a place for catalyst sulfidation through a conversion furnace, where methanol-washed acid gas, synthetic flash gas and catalyst react to sulfidate the catalyst; S3, cooling and lowering the temperature of the sulfide gas by a cooler; S4, separating the generated water through a deamination tower; S5. The separated gas is pressurized by a Roots blower and then recycled for vulcanization.
2. The method for sulfurizing methanol-washed acid gas and methanol flash gas catalyst according to claim 1, characterized in that: The specific method of sulfurization in S2 is to use N2 and CO2 as carriers, methanol-washed acid gas and methanol flash vapor as sulfurizing agents, and continuously add methanol-washed acid gas and methanol flash vapor at above 200°C, so that H2 and H2S react with CoO and MoO3 to generate CoS and MOS2.
3. The method for sulfiding methanol-washed acid gas and methanol flash gas catalyst according to claim 2, characterized in that: The reaction chemical formula of the sulfurization in S2 is: MoO3+2H2S+H2=MoS2+3H2OΔH 0 =-48.2KJ / m o CoO+H2S=CoS+H2OΔH 0 =-13.4KJ / m o。 4. The method for sulfurizing methanol-washed acid gas and methanol flash gas catalyst according to claim 1, characterized in that: The temperature rise vulcanization of the catalyst can be divided into five stages: displacement temperature rise, initial vulcanization period, main vulcanization period, final vulcanization period and temperature drop and sulfur discharge period.
5. The method for sulfiding methanol-washed acid gas and methanol flash gas catalyst according to claim 4, characterized in that: The replacement heating stage: the sulfurization heating period is an important stage during the catalyst heating and sulfurization period, which mainly evaporates the physical moisture in the catalyst layer; first, the heating process is opened, and when the nitrogen pressure added to the system is controlled at 30KPa, the heating fan is turned on, and the fan outlet pressure is controlled at about 60kPa. Depending on the nitrogen addition amount and the system outlet venting amount, the system pressure is stabilized, the catalyst air velocity is controlled to 300-500h-1, and the heating rate is about 30℃ / h (the heating rate should not exceed 50℃ / h), and the temperature is increased according to the heating curve; when the bed temperature rises to 120℃, the temperature is kept constant for about 4h to release the physical water adsorbed in the catalyst, and when the bed temperature rises to 200℃-220℃, the temperature is kept constant for about 4h to reduce the bed temperature difference, and the heating ends; a proper amount of methanol flash gas is added, and when the hydrogen content at the bed outlet is analyzed to be 5-10%, the sulfurization heating can be turned on.
6. The method for sulfurizing methanol-washed acid gas and methanol flash gas catalyst according to claim 4, characterized in that: In the initial stage of sulfidation: when the inlet temperature of the conversion furnace is greater than 220°C and the temperature of the lowest point of the catalyst layer is not less than 200°C, methanol-washed acid gas can be added, and the hydrogen sulfide concentration is 18-25% according to the requirements of the sulfuric acid production process; when the catalyst bed temperature of the conversion furnace is greater than 220°C, methanol-washed acid gas is added to the fan inlet to sulfide the catalyst, and the bed temperature rise changes are observed. The heating rate is 10-15°C / h, and the air velocity is 300-500h-1. At the beginning, the amount of acid gas added is controlled to be stable at the inlet flow rate of 50-100m3 / h; in the initial stage of sulfidation, the amount of acid gas added is slowly increased from small to large; the temperature is adjusted mainly by the electric heater and supplemented by adjusting the gas volume; the hot spot temperature in the initial stage of sulfidation shall not exceed 280°C.
7. The method for sulfurizing a methanol-washed acid gas and methanol flash gas catalyst according to claim 4, characterized in that: The main sulfurization period: when the bed temperature reaches 260-300°C, when the outlet H2S is ≥3.0g / Nm3, and the hydrogen content is greater than 5%, the main sulfurization period can be entered, the acid gas supplement at the fan inlet is increased to 100-200m3 / h, the catalyst is sulfurized, and the bed temperature is slowly raised to about 350°C and stabilized for 4 hours. If the outlet H2S is still around 10g / Nm3, the bed temperature should continue to be raised to about 400°C and kept at a constant temperature for 4 hours. If it does not reach 400°C, it can be appropriately extended for 1-2 hours to allow H2S to penetrate the catalyst bed; when H2S penetrates the bed outlet, the acid gas supplement can be increased to continue to sulfurize the catalyst, and the acid gas supplement can be increased to 1500-2000m3 / h.
8. The method for sulfurizing methanol-washed acid gas and methanol flash gas catalyst according to claim 4, characterized in that: At the end of the vulcanization, the hot spot temperature is maintained at 400-430°C, ensuring that the temperature at each point of the bed is maintained at 400-430°C for 4 hours. When the H2S at the outlet of the isothermal furnace is ≥15g / Nm3 and the hydrogen content is greater than 5%, the vulcanization is considered to be completed, the inlet and outlet valves and the vent valve are closed, and the furnace is stuffy for 4 hours.
9. The method for sulfurizing methanol-washed acid gas and methanol flash gas catalyst according to claim 4, characterized in that: The cooling and sulfur removal period: after the sulfurization is completed, gradually reduce the power of the electric heater, reduce the amount of acid gas added to cool down, close the amount of methanol flash gas, open the vent to discharge sulfur to the flare, when the temperature drops below 300°C, stop adding acid gas, increase the amount of nitrogen to continue to reduce the bed temperature to below 270°C, and when the outlet H2S is analyzed to be <1.0g / Nm3, the cooling and sulfur removal is considered to be completed, and the cooling rate is <50°C / h.
10. The method for sulfiding methanol-washed acid gas and methanol flash gas catalyst according to claim 1, characterized in that: It also includes a monitoring system for monitoring the temperature of the sulfiding gas, which includes a data acquisition module, a central processing module, a data reference module, an editing module, a communication module, a temperature control module and a gas control module.