Preparation method of CdSe / Co9S8 composite photocatalytic material

By growing CdSe on Co9S8 to form a heterojunction, the problems of photocorrosion and carrier recombination of CdSe photocatalytic materials are solved, the photocatalytic hydrogen production performance is significantly improved, and an efficient photocatalytic effect is achieved.

CN118719159AInactive Publication Date: 2024-10-01HARBIN UNIV OF SCI & TECH

Patent Information

Application Number
CN202410764239.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

CdSe photocatalytic materials suffer from severe photocorrosion and easy carrier recombination, resulting in poor performance in photocatalytic hydrogen production.

Method used

CdSe was grown on Co9S8 by solvothermal method to form a heterojunction to avoid electron-hole recombination and improve the photocatalytic performance. The specific steps include reacting in an autoclave to generate a Co9S8 precursor, then sulfiding in a sodium sulfide solution to form tubular Co9S8, and then mixing Co9S8 with the CdSe precursor solution and performing heat treatment to form a CdSe/Co9S8 composite material.

Benefits of technology

It improves the photocatalytic efficiency, extends the service life of photogenerated electrons, and significantly improves the photocatalytic hydrogen production performance. The total hydrogen production in four hours using CdSe alone is 1.1 mmol, while the total hydrogen production in four hours of the CdSe/Co9S8 composite material reaches 8.9 mmol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719159A_ABST
    Figure CN118719159A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a CdSe / Co9S8 composite photocatalytic material, and relates to the field of photocatalytic composite materials. The invention provides a method for solving the problems of low photocatalytic hydrogen production performance and low stability caused by narrow forbidden band width and high photon-generated carrier recombination rate of pure CdSe. The method comprises the following steps: 1, preparing tubular Co9S8 through a solvothermal method; and 2, growing CdSe on the surface of Co9S8 through a solvothermal method. According to the method, the CdSe / Co9S8 binary composite material is synthesized for the first time, Co9S8 is a very good photocatalytic promoter, a heterojunction is formed between CdSe and Co9S8, and Co9S8 can be beneficial to transfer of photo-induced electrons and holes of CdSe, so that the utilization rate of light is increased, and good hydrogen production performance is obtained. The method is used for preparing the composite photocatalytic material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalytic materials, and in particular to a method for preparing a CdSe / Co9S8 composite photocatalytic material. Background Art

[0002] The rapid growth of energy demand has also brought about a series of problems, the most serious of which is the resource depletion caused by the limited reserves of traditional fossil energy such as coal, oil and natural gas and their over-exploitation by humans. In recent years, hydrogen has attracted widespread attention as a high-energy-density, clean and pollution-free gas. The use of semiconductor photocatalysts for solar water splitting to produce hydrogen is a promising method for utilizing renewable resources. However, due to the problems of low sunlight utilization, easy recombination of charge-holes, and photocorrosion of photocatalysts, not all catalysts have ideal hydrogen production effects. It is very necessary to find ideal semiconductor photocatalysts.

[0003] Transition metal selenium compounds have good application prospects in many fields due to their unique electronic structure and easy synthesis, such as CdSe, ZnSe, MoSe2, etc., especially CdSe has a suitable energy band position and band gap width, has a good response to the solar spectrum, can degrade organic pollutants or photocatalytically decompose water under visible light conditions. However, CdSe also has some disadvantages, the two most prominent disadvantages are severe photocorrosion and easy recombination of carriers. Co9S8, as a low-cost co-catalyst, does not have hydrogen production performance itself, but it helps to quickly separate photogenerated carriers at the semiconductor interface. In order to solve the above problems, two or more photocatalysts are combined together to develop a composite photocatalyst. The purpose of the present invention is to grow CdSe on Co9S8 by a solvothermal method, so that Co9S8 and CdSe form a heterojunction, so that the holes of CdSe are transferred, while avoiding the recombination of electrons-holes, and promoting the photocatalytic performance of the material. Summary of the invention

[0004] The present invention mainly provides a method for solving the problem of severe photocorrosion of pure CdSe and fast recombination rate of photogenerated carriers, which leads to poor photocatalytic hydrogen production performance of CdSe, under the existing technical conditions, thereby providing a method for preparing a CdSe / Co9S8 composite photocatalytic material.

[0005] In order to solve the above problems, the present invention provides a method for preparing a CdSe / Co9S8 composite photocatalytic material, comprising the following steps:

[0006] Step S1, add 0.5-0.6 g of cobalt chloride and 0.1-0.5 g of urea to 40-60 mL of aqueous solution, stir until the particles are dissolved, transfer to an autoclave, keep warm at 100-140° C. for 9-12 hours, and when the reaction is completed, cool the autoclave to room temperature, centrifuge and wash several times with deionized water and ethanol in a centrifuge, and then dry in a vacuum drying oven overnight to obtain a purple-red precursor powder.

[0007] Step S2, disperse 0.1-0.2 g of the precursor powder prepared in S1 in 40-50 mL of deionized water, and then add 4-7 mL of sodium sulfide (4-5 M) solution under continuous stirring. At this moment, the solution gradually turns black. The obtained suspension is kept at 160-200 ° C for 20-24 h. After cooling to room temperature, it is washed with deionized water several times and then dried in a vacuum drying oven overnight to obtain tubular Co9S8.

[0008] Step S3, adding 0.004-0.009 g of selenium powder and 0.03-0.3 g of cadmium chloride pentahydrate into 14-21 mL of diethylenetriamine solvent, adding 9-14 mL of hydrazine hydrate dropwise while stirring continuously, and performing ultrasonication until completely dissolved to obtain a CdSe precursor solution.

[0009] Step S4, dissolving 0.05-0.1 g of Co9S8 prepared in S2 in an aqueous solution, then dissolving Co9S8 in 3-10 mL of an aqueous solution, and then adding it to a CdSe precursor solution, stirring for 1-2 hours, and transferring the resulting solution to a reactor lined with polytetrafluoroethylene, and keeping it at 90-130° C. for 10-15 hours. After cooling to room temperature, washing it with deionized water several times, and the centrifuge speed is 8000-10000 r / min, and finally freeze-drying it to obtain a CdSe / Co9S8 composite photocatalytic material.

[0010] Preferably, in step S1, the reaction solution is deionized water.

[0011] Preferably, in step S2, the concentration of sodium sulfide is 4-5M.

[0012] Preferably, in step S3, cadmium chloride pentahydrate is added.

[0013] Preferably, in step S4, after the CdSe precursor solution turns yellow, the Co9S8 aqueous solution is added.

[0014] Preferably, in step S4, the reaction temperature is 90-130° C., and the reaction time is 10-15 h.

[0015] Preferably, in step S4, the centrifuge speed is 8000-10000 r / min.

[0016] Preferably, in step S4, deionized water is used for centrifugal washing.

[0017] Preferably, in step S4, the drying method is freeze-drying.

[0018] In this experiment, tubular Co9S8 material was prepared by a two-step solvothermal method, and then CdSe / Co9S8 composite material was prepared by a solvothermal method. The composite of CdSe and Co9S8 materials constructs a heterojunction that can be matched, and Co9S8 can effectively help CdSe separate photogenerated carriers and improve photocatalytic efficiency. The present invention synthesizes the CdSe / Co9S8 binary complex for the first time, and a heterojunction is formed between the two, which is conducive to the transfer of CdSe photogenerated electrons and holes under sunlight irradiation, thereby improving the utilization rate of photogenerated electrons. The CdSe / Co9S8 composite material prepared by the present invention has high photocatalytic performance. A 300W xenon lamp is used as a light source, 10mg of the composite material is dissolved in 50ml of deionized water, and sodium sulfide and sodium sulfite are used as sacrificial agents to react in a reactor. The total amount of hydrogen produced by a single CdSe in four hours is 1.1mmol, while the total amount of hydrogen produced by the composite material in four hours reaches the best effect of 8.9mmol. Therefore, the CdSe / Co9S8 composite photocatalytic material prepared in the present invention has good HER performance.

[0019] On the other hand, the present invention also provides a CdSe / Co9S8 composite photocatalytic material, which is prepared by the preparation method of the CdSe / Co9S8 composite photocatalytic material as described above.

[0020] The beneficial effects of a CdSe / Co9S8 composite photocatalytic material provided by the present invention compared with the prior art are the same as the preparation method of a CdSe / Co9S8 composite photocatalytic material, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the preparation process of a CdSe / Co9S8 composite material in an embodiment of the present invention;

[0022] Figure 2 is an XRD analysis diagram of a CdSe / Co9S8 composite material in an embodiment of the present invention;

[0023] Figure 3 is a SEM image of a CdSe / Co9S8 composite material in an embodiment of the present invention;

[0024] Figure 4 This is a comparison chart of H2 production of a CdSe / Co9S8 composite material in an embodiment of the present invention; DETAILED DESCRIPTION

[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.

[0026] It should be noted that, in the absence of conflict, the features in the embodiments of the present invention can be combined with each other. The meanings of the terms "comprising", "including", "containing", and "having" are non-restrictive, that is, other steps and other ingredients that do not affect the results can be added. The above terms cover the terms "consisting of" and "essentially consisting of". Unless otherwise specified, materials, equipment, and reagents are commercially available.

[0027] The present invention provides a method for preparing a CdSe / Co9S8 composite photocatalytic material. Figure 1 As shown, the following steps are included:

[0028] Step S1, add 0.55g of cobalt chloride and 0.2g of urea to 50mL of aqueous solution, stir until the particles are dissolved, transfer to an autoclave, keep warm at 130°C for 10h, and when the reaction is completed, wait for the autoclave to cool to room temperature, centrifuge and wash several times with deionized water and ethanol in a centrifuge, and then dry in a vacuum drying oven overnight to obtain a purple-red precursor powder.

[0029] Step S2, disperse 0.12 g of the precursor powder prepared in S1 in 45 mL of deionized water, and then add 6 mL of sodium sulfide (5 M) solution under continuous stirring. At this time, the solution gradually turns black. The obtained suspension is kept at 170 ° C for 21 h. After cooling to room temperature, it is washed several times with deionized water and then dried in a vacuum drying oven overnight to obtain tubular Co9S8.

[0030] Step S3, adding 0.05 g of selenium powder and 0.14 g of cadmium chloride pentahydrate into 16 mL of diethylenetriamine solvent, adding 10 mL of hydrazine hydrate dropwise while stirring continuously, and performing ultrasonication until completely dissolved to obtain a CdSe precursor solution.

[0031] Step S4, dissolve 0.08g Co9S8 prepared in S2 in an aqueous solution, then dissolve Co9S8 in 5mL of an aqueous solution, and then add it to the CdSe precursor solution and stir for 1h. The resulting solution is transferred to a reactor lined with polytetrafluoroethylene and kept at 120°C for 10h. After cooling to room temperature, it is washed several times with deionized water at a centrifuge speed of 8000r / min, and finally freeze-dried to obtain a CdSe / Co9S8 composite photocatalytic material.

[0032] In step S1, cobalt chloride and urea are dissolved in deionized water, and the cobalt chloride and urea are fully dissolved and mixed by magnetic stirring until there are no powder particles in the solution, indicating that the solute is completely dissolved, to obtain a mixed solution, and then the mixed solution is reacted at a temperature of 100 to 140° C. and kept warm for 9 to 12 hours to allow the cobalt chloride and urea to fully react to obtain a suspension solution, and the suspension solution is centrifuged to obtain a precipitate, which is washed multiple times and then dried.

[0033] Deionized water is selected as the solvent to dissolve the hydrate of cobalt chloride and urea well, thereby ensuring that the two are fully reacted in the mixed solution. By reacting at a temperature of 100 to 140°C and keeping the temperature for 9 to 12 hours, the mixed solution can be fully reacted and the desired morphology can be obtained. After the reaction, a suspension solution containing the reaction product is obtained.

[0034] The suspended solution can be centrifuged, washed and dried to obtain a purple-red precursor material.

[0035] Specifically, the suspension solution is centrifuged at 8000-10000 r / min, and after removing the supernatant, the precipitate is washed 4-7 times with deionized water and anhydrous ethanol to remove impurities in the precipitate, and a relatively pure Co9S8 precursor is obtained. After drying at 60-90°C for 12-24 hours, a powdered Co9S8 material with a purple color is obtained. Deionized water and anhydrous ethanol are selected for washing because, on the one hand, water will not react with the reaction product, and washing with water will not introduce new impurities. On the other hand, anhydrous ethanol has good volatility and will not react with the reaction product to avoid residues in the reaction product.

[0036] In step S2, the Co9S8 precursor is dissolved in a sodium sulfide aqueous solution, and reacted at a temperature of 160 to 200°C and kept warm for 20 to 24 hours to fully sulfide the Co9S8 precursor to obtain a suspension solution. The suspension solution is centrifuged to obtain a precipitate, which is washed several times and then dried.

[0037] Specifically, the Co9S8 precursor material is reacted at 160-200° C., which can ensure complete sulfurization of the Co9S8 precursor on the one hand, and obtain a tubular Co9S8 material on the other hand. The tubular Co9S8 material is a black powder.

[0038] In step S3, selenium powder and cadmium chloride pentahydrate are added to 14-21 mL of diethylenetriamine solvent, 9-14 mL of hydrazine hydrate is added dropwise under continuous stirring, and ultrasonication is performed until the mixture is completely dissolved to obtain a CdSe precursor solution.

[0039] Here, ultrasonication is required until the solution turns yellow.

[0040] In step S4, the tubular Co9S8 material obtained in step S2 is dissolved in water, and then added to the CdSe precursor solution obtained in step S3, and mixed while adding to make the tubular Co9S8 material dispersed evenly, and avoid the accumulation of the tubular Co9S8 material, to obtain a reaction solution, and the reaction solution is transferred to a reactor, and the reaction is carried out at 90 to 130° C. for a reaction time of 10 to 15 hours. During the reaction process, selenium powder and cadmium chloride in the reaction solution react to generate CdSe, and CdSe grows on the tubular Co9S8 material to form a heterojunction.

[0041] In order to make the tubular Co9S8 material disperse more evenly, the tubular Co9S8 material can be first dissolved in water and then slowly added to the CdSe precursor solution while mixing to avoid accumulation of the tubular Co9S8 material in the reaction solution.

[0042] After the reaction is completed, the reaction solution is centrifuged, washed and dried to obtain a CdSe / Co9S8 composite photocatalytic material.

[0043] Specifically, during the centrifugation process, the speed of the centrifuge is set to 8000-10000 r / min, deionized water is used for washing 4-6 times, and after washing, freeze-drying is completed for 12-24 hours to obtain a CdSe / Co9S8 composite photocatalytic material.

[0044] Another embodiment of the present invention provides a method for preparing a CdSe / Co9S8 composite photocatalytic material, which is prepared by the method for preparing a CdSe / Co9S8 composite photocatalytic material as described above.

[0045] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on the conditions recommended by the manufacturer.

[0046] Example 1

[0047] 1.1. Add 0.55 g of cobalt chloride and 0.2 g of urea to 50 mL of aqueous solution, stir until the particles are dissolved, and then transfer to an autoclave. Keep warm at 130 ° C for 10 hours. After the reaction is completed, wait for the autoclave to cool to room temperature, centrifuge and wash several times with deionized water and ethanol in a centrifuge, and then dry in a vacuum drying oven overnight to obtain a purple-red precursor powder.

[0048] 1.2. Disperse 0.12 g of the prepared precursor powder in 45 mL of deionized water, then add 6 mL of sodium sulfide (5 M) solution under continuous stirring. At this moment, the solution gradually turns black. The obtained suspension is kept at 170 ° C for 21 h. After cooling to room temperature, it is washed several times with deionized water and then dried in a vacuum drying oven overnight to obtain tubular Co9S8.

[0049] 1.3. Add 0.04g of selenium powder and 0.14g of cadmium chloride pentahydrate into 16mL of diethylenetriamine solvent, add 10mL of hydrazine hydrate dropwise while stirring continuously, and perform ultrasonic treatment until completely dissolved to obtain a CdSe precursor solution.

[0050] 1.4. Dissolve the prepared 0.08g Co9S8 in an aqueous solution, then dissolve Co9S8 in 5mL of an aqueous solution, and then add it to the CdSe precursor solution and stir for 1h. The resulting solution is transferred to a reactor lined with polytetrafluoroethylene and kept at 120°C for 10h. After cooling to room temperature, wash it with deionized water several times at a centrifuge speed of 8000r / min. Finally, freeze-dry it to obtain a CdSe / Co9S8-6 composite photocatalytic material.

[0051] Example 2

[0052] 2.1. Add 0.55 g of cobalt chloride and 0.2 g of urea to 50 mL of aqueous solution, stir until the particles are dissolved, and then transfer to an autoclave. Keep warm at 130 ° C for 10 hours. After the reaction is completed, wait for the autoclave to cool to room temperature, centrifuge and wash several times with deionized water and ethanol in a centrifuge, and then dry in a vacuum drying oven overnight to obtain a purple-red precursor powder.

[0053] 2.2. Disperse 0.12 g of the prepared precursor powder in 45 mL of deionized water, and then add 6 mL of sodium sulfide (5 M) solution under continuous stirring. At this moment, the solution gradually turns black. The obtained suspension is kept at 170 ° C for 21 h. After cooling to room temperature, it is washed several times with deionized water and then dried in a vacuum drying oven overnight to obtain tubular Co9S8.

[0054] 2.3. Add 0.05 g of selenium powder and 0.16 g of cadmium chloride pentahydrate into 16 mL of diethylenetriamine solvent, add 10 mL of hydrazine hydrate dropwise while stirring continuously, and perform ultrasonic treatment until completely dissolved to obtain a CdSe precursor solution.

[0055] 2.4. Dissolve the prepared 0.08 g Co9S8 in an aqueous solution, then dissolve Co9S8 in 5 mL of an aqueous solution, and then add it to the CdSe precursor solution and stir for 1 h. The resulting solution is transferred to a reactor lined with polytetrafluoroethylene and kept at 120 °C for 10 h. After cooling to room temperature, wash it several times with deionized water at a centrifuge speed of 8000 r / min. Finally, freeze-dry it to obtain a CdSe / Co9S8-7 composite photocatalytic material.

[0056] Example 3

[0057] 3.1. Add 0.55 g of cobalt chloride and 0.2 g of urea to 50 mL of aqueous solution, stir until the particles are dissolved, and then transfer to an autoclave. Keep warm at 130 ° C for 10 hours. After the reaction is completed, wait for the autoclave to cool to room temperature, centrifuge and wash several times with deionized water and ethanol in a centrifuge, and then dry in a vacuum drying oven overnight to obtain a purple-red precursor powder.

[0058] 3.2. Disperse 0.12 g of the prepared precursor powder in 45 mL of deionized water, and then add 6 mL of sodium sulfide (5 M) solution under continuous stirring. At this moment, the solution gradually turns black. The obtained suspension is kept at 170 ° C for 21 h. After cooling to room temperature, it is washed several times with deionized water and then dried in a vacuum drying oven overnight to obtain tubular Co9S8.

[0059] 3.3. Add 0.06g of selenium powder and 0.18g of cadmium chloride pentahydrate into 16mL of diethylenetriamine solvent, add 10mL of hydrazine hydrate dropwise while stirring continuously, and perform ultrasonication until completely dissolved to obtain a CdSe precursor solution.

[0060] 3.4. Dissolve the prepared 0.08g Co9S8 in an aqueous solution, then dissolve Co9S8 in 5mL of an aqueous solution, and then add it to the CdSe precursor solution and stir for 1h. The resulting solution is transferred to a reactor lined with polytetrafluoroethylene and kept at 120°C for 10h. After cooling to room temperature, wash it with deionized water several times at a centrifuge speed of 8000r / min. Finally, freeze-dry it to obtain a CdSe / Co9S8-8 composite photocatalytic material.

[0061] Comparative Example 1

[0062] 4.1. Add 0.55 g of cobalt chloride and 0.2 g of urea to 50 mL of aqueous solution, stir until the particles are dissolved, and then transfer to an autoclave. Keep warm at 130 ° C for 10 h. After the reaction is completed, wait for the autoclave to cool to room temperature, centrifuge and wash several times with deionized water and ethanol in a centrifuge, and then dry in a vacuum drying oven overnight to obtain a purple-red precursor powder.

[0063] 4.2. Disperse 0.12 g of the prepared precursor powder in 45 mL of deionized water, and then add 6 mL of sodium sulfide (5 M) solution under continuous stirring. At this moment, the solution gradually turns black. The obtained suspension is kept at 170 ° C for 21 h. After cooling to room temperature, it is washed several times with deionized water and then dried in a vacuum drying oven overnight to obtain tubular Co9S8.

[0064] Comparative Example 2

[0065] 5.1. Add 0.05g of selenium powder and 0.14g of cadmium chloride pentahydrate into 16mL of diethylenetriamine solvent, add 10mL of hydrazine hydrate dropwise while stirring continuously, and perform ultrasonication until completely dissolved to obtain a CdSe precursor solution.

[0066] 5.2. Add 5 mL of deionized water to the CdSe precursor solution and stir for 1 h. Transfer the resulting solution to a reactor lined with polytetrafluoroethylene and keep it at 120°C for 10 h. After cooling to room temperature, wash it several times with deionized water at a centrifuge speed of 8000 r / min. Finally, freeze-dry it to obtain the CdSe photocatalytic material.

[0067] Experimental Example 1

[0068] The CdSe / Co9S8 composite photocatalytic materials obtained in the examples were respectively spectrally analyzed using an X'Pert PRO Cu-Kα diffractometer manufactured by Panalytical Analytical Instrument Company, wherein the scanning angle 2θ during the diffraction process was in the range of 10 to 80°.

[0069] The results are as follows Figure 2 As shown, Figure 2 The horizontal axis represents the scanning angle, and the vertical axis represents the peak intensity. Figure 2 The three curves in the middle represent Co9S8 photocatalytic materials, CdSe photocatalytic materials and CdSe / Co9S8 composite photocatalytic materials from bottom to top.

[0070] from Figure 2 It can be seen that the composite CdSe / Co9S8 sample presents diffraction peaks at 2θ values ​​of 23.90, 25.35, 27.08, 35.10, 41.96, 45.78, and 49.66, which correspond to the (100), (002), (101), (102), (110), (103), and (112) crystal planes of CdSe (JCPDS card number 08-0459). The diffraction peaks at 29.83 and 52.09 correspond to the (311) and (440) planes of Co9S8 (JCPDS card number 86-2273), respectively. XRD results show that Co9S8 and CdSe are combined together.

[0071] Experimental Example 2

[0072] The CdSe / Co9S8 composite photocatalyst material obtained in Example 1, the obtained tubular Co9S8 photocatalyst material and the CdSe photocatalyst material were characterized and observed using a field emission scanning electron microscope (FE-SEM, Sirion200, Philip).

[0073] The results are as follows Figure 3 As shown, Figure 3 (a) is the SEM image of the tubular Co9S8 photocatalytic material. Figure 3 (b) is the SEM image of CdSe photocatalytic material. Figure 3 (c) SEM image of CdSe / Co9S8 composite photocatalytic material.

[0074] from Figure 3 As can be seen from (a), the obtained Co9S8 photocatalytic material has a tubular structure; Figure 3 As can be seen from (b), the CdSe photocatalytic material obtained in Comparative Example 2 is in the shape of short rods; Figure 3 As can be seen in (c), the obtained CdSe / Co9S8 composite photocatalytic material, the short rod-shaped CdSe and the tubular Co9S8 are fully combined to form a composite material.

[0075] Experimental Example 3

[0076] The CdSe / Co9S8 composite photocatalytic material obtained in Example 1, the Co9S8 photocatalytic material obtained by comparison, and the CdSe photocatalytic material obtained by comparison were respectively used to carry out photocatalytic water decomposition and hydrogen evolution experiments to verify the performance of different materials.

[0077] The specific experimental method is: use a top-irradiated reactor with an argon lamp with a power of 300W as the reaction instrument and light source, take 10mg of CdSe / Co9S8 composite photocatalytic material, tubular Co9S8 material photocatalytic material and CdSe photocatalytic material and evenly disperse them in 50mL water, use sodium sulfide and sodium sulfite as sacrificial agents, and carry out photocatalytic hydrogen experiment at a temperature of 5°C. Every hour, the generated hydrogen is quantitatively analyzed and detected by gas chromatography, and the hydrogen production efficiency is calculated.

[0078] The results are as follows Figure 4 As shown, Figure 4 The horizontal axis represents the catalytic time, the vertical axis represents the hydrogen production, CdSe / Co9S8 represents CdSe / Co9S8 composite photocatalytic material, Co9S8 represents tubular Co9S8 photocatalytic material, and CdSe represents short rod-shaped CdSe photocatalytic material.

[0079] from Figure 4 It can be seen that after 4 hours of catalysis, the H2 production produced by the CdSe / Co9S8 composite photocatalytic material is about 8.9mmol, which is much higher than the catalytic production of tubular Co9S8 photocatalytic material (H2 production is about 0.39mmol) and CdSe photocatalytic material (H2 production is about 1.1mmol), indicating that the CdSe / Co9S8 composite photocatalytic material prepared by the method of the embodiment of the present invention can improve the photocatalytic hydrogen production performance. This is mainly because CdSe / Co9S8 has a large specific surface area, which can not only improve the light absorption rate, but also help to expose more edge positions. When CdSe particles grow in situ on the surface of tubular Co9S8 to form a composite heterojunction interface, it is beneficial to promote the migration of photogenerated electrons and reduce the recombination rate of photogenerated carriers, thereby improving the photocatalytic performance of the composite material.

[0080] In summary, the preparation method of the CdSe / Co9S8 composite photocatalytic material provided by the embodiment of the present invention, the prepared CdSe / Co9S8 composite photocatalytic material is a binary composite material, composed of tubular Co9S8 and short rod-shaped CdSe, wherein the short rod-shaped CdSe is grown in situ on the surface of the tubular Co9S8, and the two materials form a heterojunction structure at the interface. Tubular Co9S8 has a large specific surface area, thereby exposing more active sites, and CdSe is a narrow bandgap n-type semiconductor photocatalytic material with a good conduction band potential, which makes it easier to absorb visible light to form photogenerated carriers, and its conduction band potential is conducive to the decomposition and reduction of water to produce hydrogen. In addition, Co9S8, as a co-catalyst, can make the photogenerated electrons formed after CdSe is illuminated quickly transfer through the heterojunction and combine with the holes formed on the surface of Co9S8, thereby reducing the recombination rate of photogenerated carriers, which is conducive to the improvement of photocatalytic efficiency.

[0081] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing a CdSe / Co9S8 composite photocatalytic material, characterized in that The method is specifically carried out in the following steps: Step S1, add 0.5-0.6 g CoCl2·6H2O and 0.1-0.5 g urea to 40-60 mL aqueous solution, stir until the particles are dissolved, transfer to an autoclave, keep warm at 100-140° C. for 9-12 hours, and complete the reaction. After the autoclave is cooled to room temperature, wash several times by centrifugation with deionized water and ethanol in a centrifuge, and then dry in a vacuum drying oven overnight to obtain a purple-red precursor powder. Step S2, disperse 0.1-0.2 g of the precursor powder prepared in S1 in 40-50 mL of deionized water, and then add 4-7 mL of sodium sulfide (4-5 M) solution under continuous stirring. At this moment, the solution gradually turns black. The obtained suspension is kept at 160-200 ° C for 20-24 h. After cooling to room temperature, it is washed with deionized water several times and then dried in a vacuum drying oven overnight to obtain tubular Co9S8. Step S3, adding 0.04-0.09 g of selenium powder and 0.03-0.3 g of cadmium chloride pentahydrate into 14-21 mL of diethylenetriamine solvent, adding 9-14 mL of hydrazine hydrate dropwise while stirring continuously, and performing ultrasonication until completely dissolved to obtain a CdSe precursor solution. Step S4, dissolving 0.05-0.1 g of Co9S8 prepared in S2 in an aqueous solution, then dissolving Co9S8 in 3-10 mL of an aqueous solution, and then adding it to a CdSe precursor solution, stirring for 1-2 hours, and transferring the resulting solution to a reactor lined with polytetrafluoroethylene, and keeping it at 90-130° C. for 10-15 hours. After cooling to room temperature, washing it with deionized water several times, and the centrifuge speed is 8000-10000 r / min, and finally freeze-drying it to obtain a CdSe / Co9S8 composite photocatalytic material.

2. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 1, characterized in that In step S1, the reaction solution is deionized water.

3. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 1, characterized in that: In step S2, the reaction solution is a sodium sulfide aqueous solution.

4. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 1, characterized in that: In step S2, the concentration of added sodium sulfide is 4-5M.

5. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 1, characterized in that: In step S3, the selenium powder and cadmium chloride pentahydrate are completely dissolved into a yellow solution by ultrasound.

6. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 1, characterized in that: In the step S4, the reaction temperature is 90-130° C. and the reaction time is 10-15 h.

7. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 1, characterized in that: In step S4, the centrifuge speed is 8000-10000 r / min.

8. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 1, characterized in that: In step S4, deionized water is used for centrifugal washing.

9. The method for preparing a CdSe / Co9S8 composite photocatalytic material according to claim 8, characterized in that: In step S4, the drying method is freeze drying.

10. A method for preparing a CdSe / Co9S8 composite photocatalytic material, characterized in that: The photocatalytic material is prepared by the method for preparing the CdSe / Co9S8 composite photocatalytic material as described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Co9S8-MoS2 g-C3N4 loaded electrocatalytic hydrogen production catalyst and preparation method thereof

    CN111545238A

  • Preparation method of carbon-dot-assisted Zn-AgIn5S8 / Co9S8 quantum dot and application of carbon-dot-assisted Zn-AgIn5S8 / Co9S8 quantum dot in photohydrolysis hydrogen production

    CN113368876A

  • Co9S8 / ZnIn2S4 photocatalytic hydrogen production material as well as preparation method and application thereof

    CN113751029A

  • Tubular In2O3 / CdSe composite photocatalytic material and preparation method thereof

    CN115501892A

  • Preparation method and application of CdSe / KTaO3 composite photocatalyst

    CN117160493A

Cited By

  • Bimetal sulfide modified cadmium selenide photocatalyst as well as preparation method and application thereof