Production method for solving annealing blistering of double-zero aluminum foil
By controlling the plate shape, residual rolling oil amount and coiling density during the aluminum foil rolling and annealing processes, and performing low-temperature insulation and slow temperature rise, the problem of blistering during double-zero aluminum foil annealing is solved and product quality and performance are improved.
Patent Information
- Application Number
- CN202411223276.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Double-zero aluminum foil often bubbles during the annealing process, which affects product quality and customer experience. Existing methods cannot completely eliminate it and cause waste. A new production method is needed to solve this problem.
During the aluminum foil rolling process, the flatness of the plate shape and the amount of residual rolling oil on the surface are controlled, the coiling density is controlled during slitting, and low-temperature insulation and slow heating are performed before annealing to control the volatilization of the rolling oil and the heat transfer of the aluminum foil. strain.
It effectively controls the volatilization of rolling oil and the thermal strain of aluminum foil, significantly improves the quality and performance of double-zero aluminum foil, avoids blistering, and reduces waste.
Smart Images

Figure CN118719804A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultra-thin aluminum alloy foil production, and in particular to a production method for solving blistering during annealing of double-zero aluminum foil. Background Art
[0002] As a lightweight, high-strength, environmentally friendly, non-toxic, odorless, and recyclable material, double-zero aluminum foil offers excellent sealing, waterproofing, light-proofing, and oxygen-barrier properties, making it widely used in packaging for food, medicine, and electronic devices. Currently, aluminum foil, especially double-zero aluminum foil, is primarily manufactured domestically and internationally using 1000 and 8000 series aluminum alloys (such as 1235, 8111, and 8079). It is used in food packaging for milk, beverages, and solid foods, pharmaceutical packaging for capsules, tablets, and syringes, and electronic component packaging, as well as thermal insulation and construction applications.
[0003] Currently, there are two common production processes for double-zero aluminum foil: one is "using hot-rolled billet - cold rolling - foil rolling - slitting - annealing - packaging" and the other is "using cast-rolled billet - cold rolling - foil rolling - slitting - annealing - packaging." The finished aluminum foil produced using either process will exhibit varying degrees of "bubbles" on both sides of the foil roll during the lamination process, a phenomenon known in the industry as "annealing blistering" (see attached for details on blistering). Figure 2 (The left image, difficult to observe due to the extremely bright aluminum foil, appears primarily on the outer layer of the roll and is more pronounced with thinner foil.) This annealing blistering can cause wrinkling during lamination with other materials, seriously impacting product quality and customer experience.
[0004] After extensive research, it was found that during the rolling process, a layer of rolling oil film will remain on the surface of the aluminum foil; during the slitting process, the aluminum foil will be cut into single aluminum foil rolls according to a certain winding density. There will be a certain gap between the layers of aluminum foil, and this gap is filled with residual rolling oil from the rolling process; during annealing and heating, the rolling oil can only evaporate from the end surface of the aluminum foil roll through the gap between the layers. However, the gap between the layers is not a flat gap, but more like a porous structure. The surface roughness of aluminum foil is generally 0.15-0.35μm, and the gap between the layers of aluminum foil is also less than 1μm according to measurement and calculation. Therefore, the gap between the layers is staggered at the microscopic level (see Appendix). Figure 1), which greatly complicates the oil and gas diffusion path. During the annealing process, especially after rapid heating, the oil film expands dramatically, transforming into an oil-gas cluster, which generates tremendous pressure. However, once the rolling oil becomes vaporized, it cannot evaporate smoothly from the gaps. Instead, it is squeezed out of the gaps, causing the aluminum foil to deform and form blistering. Therefore, many factors influence annealing blistering, including the rolled plate shape, the amount of rolling oil residue on the surface of the finished aluminum foil, the slitting and coiling density, and the annealing heating rate.
[0005] To address the issue of blistering during the annealing of double-zero aluminum foil, the aluminum foil industry typically controls this by stripping off the outer layer of the foil roll. However, this method fails to completely eliminate blistering and results in significant waste. Therefore, a new and effective production method is needed to address this issue. Currently, no method has been reported to address this issue during the production process. Summary of the Invention
[0006] In the production process of aluminum foil, whether hot-rolled billets or cast-rolled billets are used, foil rolling, slitting and annealing must be carried out after cold rolling, and finally packaged as finished products. In order to overcome the above-mentioned shortcomings of the prior art, the present invention provides a production method for solving the blistering of double-zero aluminum foil during annealing, thereby improving the quality and performance of double-zero aluminum foil.
[0007] The purpose of the present invention is achieved through the following technical solutions: A production method for solving blistering during annealing of double-zero aluminum foil according to the present invention comprises the following steps: S1, during the aluminum foil rolling process, controls the flatness of the aluminum foil in the intermediate rolling passes and the finished rolling passes; S2, when rolling the finished product, control the residual rolling oil on the surface of the aluminum foil to ≤17mg / m 2 ; S3, during slitting and coiling, control the coiling density of the slitting aluminum foil roll to be between 2.32 and 2.46 g / cm³; S4. During the annealing process, first heat the material from room temperature to 70-90°C, then keep the temperature for 12-24 hours; then heat the material to the annealing temperature for annealing, and the heating rate should be controlled at 3-15°C / h.
[0008] In the aluminum alloy plate and strip processing industry, the indicator for evaluating the plate quality is expressed as "straightness". In order to control the good straightness of the aluminum foil, the aluminum foil is divided into four positions along the width direction according to the principle of symmetry during the actual processing process, namely the plate shape one, plate shape two, plate shape three, and plate shape four (see Plate Shape Settings Figure 3Flatness 1 refers to the flatness value at the middle position along the width direction of the aluminum foil. A positive value indicates that the middle is loose, while a negative value indicates that the middle is tight. Flatness 2 refers to the flatness inclination value at both sides along the width direction of the aluminum foil. A positive value indicates that the operating side is tighter than the transmission side, while a negative value indicates that the operating side is looser than the transmission side. Flatness 3 refers to the flatness index at both sides of the aluminum foil along the width direction. A positive value indicates that both sides are tight, while a negative value indicates that both sides are loose. Flatness 4 refers to the flatness value at the second rib position along the width direction of the aluminum foil. A positive value indicates that the second rib is loose, while a negative value indicates that the second rib is tight.
[0009] The unit of straightness is "I", that is, 1 "I" unit is defined as the straightness error caused by 0.001% or 1 part in 100,000 of the difference in fiber length between the strips. In other words, if a 1000mm long strip is rolled and its edge length is 1000.01mm, the straightness error between the center and the edge will be 1 "I" unit. Preferably, the straightness settings for the intermediate rolling passes are: shape one is -12I to -2I, shape two is 0I, shape three is -4I to -1I, and shape four is 0I; the flatness settings for the finished rolling passes are: shape one is -28I to -12I, shape two is 0I, shape three is -6I to -2I, and shape four is 0I; the shape of the finished aluminum foil is measured on an offline shape meter, and the sagging of the two edges is controlled within a range of -8 to -2mm.
[0010] Preferably, in order to control the amount of rolling oil remaining on the surface of the aluminum foil, in step S2, the surface purge pressure of the outlet aluminum foil of the finished rolling pass can be set to 0.2-0.5 MPa to purge away excess rolling oil.
[0011] In this industry, winding density = actual coil weight / actual volume. Due to the gaps between layers, the winding density will be lower than the metal density of the aluminum foil. If the winding density is too high, it will not be conducive to the volatilization of the rolling oil and will more easily cause annealing blistering. If the winding density is too low, the aluminum foil roll will be unstable and prone to misalignment or pitting. Preferably, in order to accurately control the winding density of the slit aluminum foil roll, it is necessary to control the winding tension to 22-40MPa, the support roller pressure to 2.0-3.0N / mm, the flattening roller pressure to 1.0-2.0N / mm, and the surface tension to 10MPa.
[0012] The aluminum foil coil of the present invention is maintained at 70-90°C for 12-24 hours before formal annealing. This allows some of the rolling oil at the edge of the foil to evaporate at this temperature. Furthermore, the foil's strength remains relatively stable at this temperature, and the oil vaporization and volatilization process does not cause deformation. Preferably, the heating rate at each stage of the annealing process is controlled to be: 10-15°C / h for 0.007-0.009 mm aluminum foil; 6-10°C / h for 0.0058-0.007 mm aluminum foil; and 3-6°C / h for 0.0045-0.0058 mm aluminum foil.
[0013] Compared with the prior art, the present invention has the following positive effects: The method of the present invention can effectively control the volatilization of rolling oil in the annealing process, solve the problem of extrusion deformation of aluminum foil caused by the huge pressure generated by the vaporization of rolling oil, and can significantly improve the quality and performance of double-zero aluminum foil: through precise plate shape control, the "cloth bag tied mouth" effect formed by the tight edges of the aluminum foil roll during the winding process is improved, so that the aluminum foil rolling oil is more likely to evaporate without generating huge pressure inside the aluminum foil roll; strict surface residual oil control reduces the pressure generated by the vaporization of residual rolling oil; reasonable slitting and coiling density control helps to maintain the structural stability of the aluminum foil and is conducive to the volatilization of rolling oil from the middle to the end surface of the aluminum foil roll; precise rolling oil volatilization control allows a portion of the rolling oil on both sides of the aluminum foil roll to evaporate before the performance of the aluminum foil is reduced, which is conducive to the pressure stability of the subsequent rolling oil volatilization process from the inside of the roll to the outside. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a microscopic diagram of the layers of aluminum foil roll.
[0015] Figure 2 It is the annealing blister that occurs in aluminum foil coils produced by conventional production methods.
[0016] Figure 3 It is a schematic diagram of plate flatness and its setting. DETAILED DESCRIPTION
[0017] The present invention will be further described below through specific embodiments, which are only used to illustrate the present invention rather than to limit the present invention.
[0018] Example 1
[0019] Aluminum foil with a thickness of 0.006 mm and a width of 1626 mm is produced using cast and rolled 8079 aluminum alloy. The production process is "cold rolling - foil rolling - slitting - annealing - packaging". The production method for solving the blistering of double-zero aluminum foil during annealing is adopted, including the following steps: S1. During the foil rolling process, the straightness of the aluminum foil shape in the intermediate rolling passes and the finished rolling passes is controlled: the flatness of the intermediate rolling pass is set as: shape one is -8I, shape two is 0I, shape three is -2I, and shape four is 0I; the flatness of the finished rolling pass is set as: shape one is -18I, shape two is 0I, shape three is -3I, and shape four is 0I; after the aluminum foil is rolled in the finished pass, the shape is measured on an offline shape meter, and the sagging on both sides is -4.2mm.
[0020] S2, when the aluminum foil is rolled into finished products, the surface purge pressure of the outlet aluminum foil is set to 0.32MPa. The surface residual oil of the rolled aluminum foil is measured and the residual rolling oil on the surface of the aluminum foil is controlled to be 13.8mg / m 2 .
[0021] In step S3, the finished rolled aluminum foil coil is moved to the slitting machine for slitting. The coiling tension during the slitting process is set to 30 MPa, the support roller pressure is 2.4 N / mm, the flattening roller pressure is 1.5 N / mm, and the surface tension is 6 MPa. The density of the slit aluminum foil coil is measured in real time, and the actual coiling density of the aluminum foil coil is 2.43 g / cm³.
[0022] S4: Place the slit aluminum foil rolls into an annealing furnace. Set the heating rate to 7.5°C / h, first raise the temperature from room temperature to 80°C, and then keep it at that temperature for 16 hours. Then, raise the temperature to the annealing temperature at the same heating rate, and anneal according to the conventional process until the annealing is completed.
[0023] The annealed aluminum foil roll was moved to the rewinding machine for rewinding inspection. No annealing blistering was found, indicating good quality.
[0024] Comparative Example 1 Comparative Example 1 is a comparative example of Example 1, except that in S3, the finished rolled aluminum foil coil is moved to a slitting machine for slitting. During the slitting process, the winding tension is set to 43 MPa, the support roller pressure is 3.2 N / mm, the flattening roller pressure is 2.5 N / mm, and the surface tension is 6 MPa. The density of the aluminum foil coil after slitting is measured in real time, and the actual winding density is 2.53 g / cm³.
[0025] The annealed aluminum foil roll was moved to the rewinding machine for rewinding inspection. Within 1,000 meters of the rewinding outer circle, intermittent annealing blistering occurred 39 times, and the annealing blister quality problem was not solved.
[0026] Example 2
[0027] Aluminum foil with a thickness of 0.0055 mm and a width of 1460 mm is produced using hot-rolled 8079 aluminum alloy. The production process is "cold rolling - foil rolling - slitting - annealing - packaging". The production method for solving the blistering of double-zero aluminum foil during annealing is adopted, which includes the following steps: S1. During the foil rolling process, the straightness of the aluminum foil shape in the intermediate rolling passes and the finished rolling passes is controlled: the flatness of the intermediate rolling pass is set to: shape one is -9I, shape two is 0I, shape three is -2I, and shape four is 0I; the flatness of the finished rolling pass is set to: shape one is -20I, shape two is 0I, shape three is -3I, and shape four is 0I; after the aluminum foil is rolled in the finished pass, the shape is measured on an offline shape meter, and the sagging on both sides is -4.7mm.
[0028] S2, when the aluminum foil is rolled into finished products, the surface purge pressure of the outlet aluminum foil is set to 0.28MPa. The surface residual oil of the rolled aluminum foil is measured and the residual rolling oil on the surface of the aluminum foil is controlled to be 15.2mg / m 2 .
[0029] In step S3, the finished rolled aluminum foil coil is moved to the slitting machine for slitting. The coiling tension during the slitting process is set to 33 MPa, the support roller pressure is 2.4 N / mm, the flattening roller pressure is 1.5 N / mm, and the surface tension is 6 MPa. The density of the slit aluminum foil coil is measured in real time, and the actual coiling density of the aluminum foil coil is 2.41 g / cm³.
[0030] S4: Place the slit aluminum foil roll into an annealing furnace, set the heating rate at 5.0°C / h, first raise the temperature from room temperature to 80°C, and then keep it at this temperature for 16 hours; then raise the temperature to the annealing temperature at the same heating rate, and anneal according to the conventional process until the annealing is completed.
[0031] The annealed aluminum foil roll was moved to the rewinding machine for rewinding inspection. No annealing blistering was found, indicating good quality.
[0032] Comparative Example 2 Comparative Example 2 is a comparative example of Example 2, except that in S2, when the aluminum foil is rolled into the finished product, the surface purge pressure of the outlet aluminum foil is set to 0.18 MPa. The surface residual oil of the rolled aluminum foil is measured and the residual rolling oil on the surface of the aluminum foil is controlled to be 21.4 mg / m 2 ;The actual aluminum foil roll density is 2.40g / cm³.
[0033] The annealed aluminum foil roll was moved to the rewinding machine for rewinding inspection. Within 1,000 meters of the rewinding outer circle, intermittent annealing blistering occurred 57 times, and the annealing blister quality problem was not solved.
[0034] Example 3
[0035] Aluminum foil with a thickness of 0.0053 mm and a width of 1240 mm is produced using cast and rolled 8079 aluminum alloy. The production process is "cold rolling - foil rolling - slitting - annealing - packaging". The production method for solving the blistering of double-zero aluminum foil during annealing is adopted, including the following steps: S1. During the foil rolling process, the straightness of the aluminum foil shape in the intermediate rolling passes and the finished rolling passes is controlled: the flatness of the intermediate rolling pass is set as: shape one is -6I, shape two is 0I, shape three is -2I, and shape four is 0I; the flatness of the finished rolling pass is set as: shape one is -16I, shape two is 0I, shape three is -4I, and shape four is 0I; after the aluminum foil is rolled in the finished pass, the shape is measured on an offline shape meter, and the sagging on both sides is -3.1mm.
[0036] S2, when the aluminum foil is rolled into finished products, the surface purge pressure of the outlet aluminum foil is set to 0.3MPa. The surface residual oil of the rolled aluminum foil is measured and the residual rolling oil on the surface of the aluminum foil is controlled to be 14.2mg / m 2 .
[0037] In step S3, the finished rolled aluminum foil coil is moved to the slitting machine for slitting. The coiling tension during the slitting process is set to 34 MPa, the support roller pressure is 2.4 N / mm, the flattening roller pressure is 1.5 N / mm, and the surface tension is 6 MPa. The density of the slit aluminum foil coil is measured in real time, and the actual coiling density of the aluminum foil coil is 2.42 g / cm³.
[0038] S4: Place the slit aluminum foil roll into an annealing furnace, set the heating rate at 5.0°C / h, first raise the temperature from room temperature to 80°C, and then keep it at this temperature for 16 hours; then raise the temperature to the annealing temperature at the same heating rate, and anneal according to the conventional process until the annealing is completed.
[0039] The annealed aluminum foil roll was moved to the rewinding machine for rewinding inspection. No annealing blistering was found, indicating good quality.
[0040] Comparative Example 3 Comparative Example 3 is a comparative example of Example 3, except that: S1. During the foil rolling process, the straightness of the aluminum foil shape in the intermediate rolling passes and the finished rolling passes is controlled: the flatness of the intermediate rolling pass is set to: shape one is -6I, shape two is 0I, shape three is -2I, and shape four is 0I; the flatness of the finished rolling pass is set to: shape one is -10I, shape two is 0I, shape three is 0I, and shape four is 0I; after the aluminum foil is rolled in the finished pass, the shape is measured on an offline shape meter, and the sagging on both sides is -3.1mm.
[0041] In step S3, the finished rolled aluminum foil coil is moved to the slitting machine for slitting. The coiling tension during the slitting process is set to 43 MPa, the support roller pressure is 3.2 N / mm, the flattening roller pressure is 2.5 N / mm, and the surface tension is 6 MPa. The density of the slit aluminum foil coil is measured in real time, and the actual coiling density is 2.52 g / cm³.
[0042] The aluminum foil roll that has completed annealing was moved to the rewinding machine for rewinding inspection. Within 1,000 meters of the outer circle of the rewinding, intermittent annealing blistering occurred 74 times, and the annealing blister quality problem was not solved.
[0043] Example 4
[0044] Aluminum foil with a thickness of 0.009 mm and a width of 1510 mm is produced using hot-rolled 8079 aluminum alloy. The production process is "cold rolling - foil rolling - slitting - annealing - packaging". The production method for solving the blistering of double-zero aluminum foil during annealing is adopted, which includes the following steps: S1. During the foil rolling process, the straightness of the aluminum foil shape in the intermediate rolling passes and the finished rolling passes is controlled: the flatness of the intermediate rolling pass is set to: shape one is -7I, shape two is 0I, shape three is -3I, and shape four is 0I; the flatness of the finished rolling pass is set to: shape one is -19I, shape two is 0I, shape three is -3I, and shape four is 0I; after the aluminum foil is rolled in the finished pass, the shape is measured on an offline shape meter, and the sagging on both sides is -4.3mm.
[0045] S2, when the aluminum foil is rolled into finished products, the surface purge pressure of the outlet aluminum foil is set to 0.32MPa. The surface residual oil of the rolled aluminum foil is measured and the residual rolling oil on the surface of the aluminum foil is controlled to be 14.3mg / m 2 .
[0046] In step S3, the finished rolled aluminum foil coil is moved to the slitting machine for slitting. During the slitting process, the coiling tension is set to 28 MPa, the support roller pressure is 2.5 N / mm, the flattening roller pressure is 1.4 N / mm, and the surface tension is 7 MPa. The density of the slit aluminum foil coil is measured in real time, and the actual coiling density of the aluminum foil coil is 2.42 g / cm³.
[0047] S4: Place the slit aluminum foil roll into an annealing furnace and set the heating rate at 12.0°C / h. First, heat it from room temperature to 80°C and then keep it at that temperature for 18 hours. Then, heat it to the annealing temperature at the same heating rate and anneal it according to the conventional process until the annealing is completed.
[0048] The annealed aluminum foil roll was moved to the rewinding machine for rewinding inspection. No annealing blistering was found, indicating good quality.
[0049] Comparative Example 4 Comparative Example 4 is a comparative example of Example 4, except that: S1. During the foil rolling process, the straightness of the aluminum foil shape in the intermediate rolling passes and the finished rolling passes is controlled: the flatness of the intermediate rolling pass is set as: shape one is -7I, shape two is 0I, shape three is -3I, and shape four is 0I; the flatness of the finished rolling pass is set as: shape one is -9I, shape two is 0I, shape three is -1I, and shape four is 0I; after the aluminum foil is rolled in the finished pass, the shape is measured on an offline shape meter, and the sagging on both sides is -1.2mm.
[0050] S4: Place the slit aluminum foil roll into an annealing furnace, set the heating rate at 17.0°C / h, first raise the temperature from room temperature to 80°C, and then keep it at this temperature for 10 hours; then raise the temperature to the annealing temperature at the same heating rate, and anneal according to the conventional process until the annealing is completed.
[0051] The annealed aluminum foil roll was moved to the rewinding machine for rewinding inspection. Within 1,000 meters of the outer rewinding circle, intermittent annealing blistering occurred 44 times, and the annealing blister quality problem was not solved.
Claims
1. A production method for solving the blistering of double zero aluminum foil annealing, characterized in that: The following steps are involved: S1, during the aluminum foil rolling process, controls the flatness of the aluminum foil in the intermediate rolling pass and the finished rolling pass; S2, when rolling the finished product, control the residual rolling oil on the surface of the aluminum foil to ≤17mg / m 2 ; S3, when slitting and coiling, control the coiling density of the slitting aluminum foil coil to be between 2.32 and 2.46 g / cm³; S4, during the annealing process, first raise the temperature from room temperature to 70-90°C, then keep it at this temperature for 12-24h; then raise the temperature to the annealing temperature for annealing, and the heating rate should be controlled at 3-15°C / h.
2. The production method for solving the blistering of double zero aluminum foil annealing according to claim 1 is characterized in that: The flatness setting of the intermediate rolling pass is: plate shape one is -12I~-2I, plate shape two is 0I, plate shape three is -4I~-1I, and plate shape four is 0I; the flatness setting of the finished rolling pass is: plate shape one is -28I~-12I, plate shape two is 0I, plate shape three is -6I~-2I, and plate shape four is 0I; the shape of the aluminum foil of the finished pass is measured on the offline shape meter, and the control range of the sag on both sides is -8~-2mm.
3. The production method for solving the blistering of double zero aluminum foil annealing according to claim 1 is characterized in that: In step S2, the surface purge pressure of the outlet aluminum foil of the finished rolling pass is 0.2-0.5 MPa.
4. The production method for solving the blistering of double zero aluminum foil annealing according to claim 1 is characterized in that: In step S3, the winding tension of the slit aluminum foil roll is 22-40 MPa, the support roller pressure is 2.0-3.0 N / mm, the flattening roller pressure is 1.0-2.0 N / mm, and the surface tension is 1-10 MPa.
5. The production method for solving the blistering of double zero aluminum foil annealing according to claim 1 is characterized in that: During the annealing process, the heating rate of each heating stage should be controlled: the heating rate of 0.007-0.009 mm aluminum foil is 10-15°C / h; the heating rate of 0.0058-0.007 mm aluminum foil is 6-10°C / h; the heating rate of 0.0045-0.0058 mm aluminum foil is 3-6°C / h.
Citation Information
Patent Citations
Annealing process for aluminum foil
CN102560294A
Finished product annealing process for double zero aluminum foils
CN106521372A
Annealing process capable of preventing surface hot bulging for light gauge foil
CN109811283A
Method for inhibiting annealing hot bulging of double-zero foil
CN115125459A
Aluminum foil, method for producing the same and use thereof