Multi-furnace continuous casting method for continuous casting of high-aluminum steel with ultrahigh aluminum content

By using a high thermal conductivity barrier layer and liquid mold slag in high-aluminum steel continuous casting, the problems of strong slag-steel reaction and low slag consumption in high-aluminum steel continuous casting are solved, and multi-furnace continuous pouring and slab quality improvement are achieved. stability.

CN118720076AActive Publication Date: 2024-10-01ANGANG STEEL CO LTD +1

Patent Information

Application Number
CN202410846275.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-01
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

In the continuous casting process of high-aluminum steel, the traditional CaO-Al2O3-based mold slag has problems such as strong crystallization performance, low slag consumption, unstable slab surface quality caused by reactive components, and strong slag-steel reaction, which affects continuous casting. The process goes smoothly.

Method used

A barrier layer with high thermal conductivity, high temperature resistance, and anti-oxidation is added to the contact surface between the mold slag and the molten steel to reduce the contact area, and liquid mold slag is added directly into the mold to ensure stable slag consumption and lubrication and heat transfer functions.

Benefits of technology

It effectively suppresses the slag-steel reaction, improves the quality of the cast slab, realizes continuous pouring in multiple furnaces, and solves the problems of low slag consumption and bonded steel leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720076A_ABST
    Figure CN118720076A_ABST
Patent Text Reader

Abstract

The invention relates to a multi-furnace continuous casting method for continuous casting of ultrahigh-aluminum-content high-aluminum steel. The method comprises the steps of heating of a blocking device and a crystallizer cover plate, preparation of liquid protection liquid, putting of the blocking device on the surface of molten steel and covering of the crystallizer cover plate in the continuous casting process, injection of liquid protection slag, control of the flow speed of the liquid protection slag and the like. A blocking layer with the characteristics of high heat conductivity, high temperature resistance and oxidation resistance is additionally arranged on the contact surface of the casting powder and molten steel, so that the contact area of the molten steel and the casting powder is reduced, and the slag-steel reaction capacity is inhibited; on the basis, liquid casting powder is directly added into the crystallizer, so that the casting powder is ensured to flow into a slag channel, the slag consumption of the high-aluminum steel during continuous casting production is stabilized, and meanwhile, the casting powder has stable lubrication and heat transfer functions; a series of problems that slag-steel reaction is strong, casting powder is easy to crystallize and separate out slag strips, slag consumption is low, bonding breakout is easy to occur and the like during continuous casting production of the ultrahigh-aluminum-content high-aluminum steel are solved, and multi-furnace continuous casting of the type of steel is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous casting, and in particular to a multi-furnace continuous casting method for continuous casting of high-aluminum steel with ultra-high aluminum content (Al≥4%). Background Art

[0002] Increasing the Al content in steel can greatly improve the performance of steel, such as aluminum-containing TRIP steel, TWIP steel, etc., which are important materials for achieving lightweight automobiles. However, Al in molten steel is an active element. When using traditional CaO-SiO2-based protective slag casting process, Al will react with SiO2 and other components in the protective slag to form a slag-steel reaction, causing changes in the composition and performance of the protective slag, resulting in the inability to smoothly carry out the continuous casting process. Therefore, with the gradual increase of aluminum content in high-aluminum steel products, it has brought great challenges to the traditional continuous casting process.

[0003] Based on the above problems, some researchers have developed a new type of high-aluminum steel continuous casting protective slag, which mainly includes two categories: low-basicity CaO-SiO2-based protective slag and low-reactivity CaO-Al2O3-based protective slag. In practical applications, low-basicity CaO-SiO2-based protective slag can meet the continuous casting production of high-aluminum steel (aluminum content less than 1%) with low slag-steel reaction intensity. In the production of steel grades with higher aluminum content, low-reactivity CaO-Al2O3-based protective slag has shown better potential.

[0004] A domestic factory used low-basicity CaO-SiO2-based protective slag and low-reactivity CaO-Al2O3-based protective slag to carry out continuous casting production tests of high-aluminum steel with an aluminum content of 4%, and both encountered the problem of difficulty in single-furnace casting. Therefore, how to optimize the continuous casting production process of high-aluminum steel with ultra-high aluminum content (Al≥4%), further inhibit the slag-steel reaction, stabilize the physical and chemical properties of the protective slag, so as to stably obtain good ingot quality and ensure the smooth operation of the continuous casting process is an urgent problem to be solved.

[0005] The Chinese patent application with publication number CN108213365A discloses "a non-reactive protective slag for high aluminum steel", the weight percentage of which is CaO: 26% to 40%, Al2O3: 18% to 28%, BaO: 14% to 28%, Li2O: 2% to 10%, F: 6% to 14%, MgO≤2%, C: 2% to 8%, and the rest are inevitable impurities, and the impurities (Na2O+K2O+SiO2) are kept ≤2%. The protective slag basically does not contain SiO2, Na2O, Fe2O3, B2O3 and other components that react with active elements such as Al and Ti in molten steel. After use, the protective slag composition and performance remain stable, which can ensure the smoothness of the high aluminum steel continuous casting process. However, the crystallization ability of the protective slag is too strong, and the crystallization rate reaches 100%; at the same time, the Li2O content is too high, and the protective slag is expensive.

[0006] The Chinese patent application with publication number CN114130972A discloses "a non-reactive protective slag for continuous casting crystallizer of fluorine-free high-aluminum steel", which includes CaO: 20-35%, Al2O3: 15-35%, SiO2: 1-10%, BaO: 7-15%, B2O3: 7-15%, Na2O+Li2O: 10-17%, C: 2-10%, MnO: 1-7%, and MgO: 1-7%, and the rest are inevitable impurities. SiO2, B2O3 and Na2O in the protective slag are still reactive with Al in molten steel.

[0007] The Chinese patent application with publication number CN106270429A discloses "a low-reactivity mold slag and preparation method thereof", which contains SiO2: 8±2%, CaO: 32-38%, Al2O3: 25-31%, MgO: 1-5%, Na2O: 6-10%, F: 4-8%, Li2O: 1-4%, BaO: 0-6%, B2O3: 1-4%, C: 1-5% and inevitable impurities by mass percentage. It limits the content of silicon dioxide in the mold slag to a stable content range, reducing the slag-steel reaction characteristics of the mold slag, but the Na2O and B2O3 contained in it still have strong reactivity with Al in molten steel.

[0008] The Chinese patent application with publication number CN102764866A discloses "a kind of high Al2O3 content high aluminum steel continuous casting protection slag", the chemical composition of the protection slag is as follows by mass percentage: CaO: 5-20%, BaO: 5-20%, Al2O3: 20-50%, B2O3: 2-15%, SiO2≤7%, flux: CaF2: 6-13%, Na2O: 6-13%, Li2O: 1-4%, MnO: 2-6%, C: 3-10%. The protection slag has a good glass morphology and can greatly reduce the reaction between aluminum in steel and SiO2 in the slag. However, the protection slag contains Na2O and B2O3, and the above components are still reactive with Al in molten steel.

[0009] It can be seen that the main method to solve the problem of strong slag-steel reaction during the continuous casting of high-aluminum steel is to use low-reactivity protective slag with CaO-Al2O3 as the slag-based component. However, there are always two problems that are difficult to solve with CaO-Al2O3-based protective slag: (1) The crystallization performance of CaO-Al2O3-based protective slag is strong, the slag consumption in actual application is low, and the surface quality of the produced ingot is unstable; (2) There are other flux components in the CaO-Al2O3-based protective slag that are reactive with Al in the molten steel, such as Na2O, B2O3, etc., which are reactive with molten steel with a high Al content, resulting in changes in the composition and performance of the protective slag, affecting the smooth operation of the continuous casting process.

[0010] The Chinese utility model patent with publication number CN205732868U discloses "a crystallizer cover plate device for pouring liquid protective slag", including: a cover plate, at least two ring tubes and an argon blowing tube. The cover plate with a molten steel pouring hole and a slag conveying hole is arranged at the upper end of the crystallizer; the cover plate is a sandwich structure; the cover plate is coated with a high-temperature radiation coating on the side close to the molten steel. At least two ring tubes are respectively embedded in the bottom outer edges of the molten steel pouring hole and the slag conveying hole; a plurality of through holes are opened at the bottom of the ring tube; the argon blowing tube is connected to the top of the ring tube. The crystallizer cover plate device can isolate the air, prevent the secondary oxidation of the molten steel, improve the thermal insulation performance of the crystallizer, increase the temperature of the molten steel on the meniscus, reduce the depth of vibration marks, avoid the formation of solidification hooks, reduce pinholes and reduce the adhesion of liquid slag on the meniscus, and ultimately improve the quality of the ingot.

[0011] The Chinese utility model patent with publication number CN205341853U discloses "a conveying device for liquid protective slag for continuous casting". The slag conveying pipe includes: an inner pipe, a protective layer and a heating element; the hollow cylindrical inner pipe is made of graphite; the protective layer is wrapped outside the inner pipe; and the heating element is arranged outside the protective layer. The conveying device includes: a slag conveying pipe, a slag storage device and a throttle valve; the slag storage device is a hollow cylinder with an opening at one end; the slag storage device is wrapped with a second protective layer; a second heating element is arranged outside the second protective layer; the slag inlet of the slag conveying pipe is connected and fixed to the closed end of the slag storage device, and the slag outlet of the slag conveying pipe is arranged on the side of the submerged water inlet of the crystallizer; the throttle valve is arranged at the slag inlet of the slag conveying pipe, which plays the role of a gate flow storage. The conveying device enables the liquid protective slag to quickly and evenly cover the surface of the molten steel in the crystallizer and fill the gap between the solidified billet shell and the wall of the crystallizer, which can effectively improve the surface quality of the ingot.

[0012] The above two technical solutions are devices for directly adding liquid protective slag into the continuous casting crystallizer. Currently, this technical means has received more attention and is a new research and development direction. Summary of the invention

[0013] The present invention provides a method for continuous casting of high-aluminum steel with ultra-high aluminum content by multiple furnaces. A blocking layer with high thermal conductivity, high temperature resistance and oxidation resistance is added on the contact surface between the protective slag and molten steel to reduce the contact area between the molten steel and the protective slag and inhibit the reaction ability of the slag-steel. On this basis, liquid protective slag is directly added into the crystallizer to ensure that the protective slag flows into the slag channel, stabilizes the slag consumption of the high-aluminum steel during continuous casting production, and ensures that the protective slag has stable lubrication and heat transfer functions, solves a series of difficult problems in the continuous casting production of high-aluminum steel with ultra-high aluminum content, such as strong slag-steel reaction, easy crystallization of protective slag to precipitate slag strips, low slag consumption, easy adhesion and steel leakage, etc., and realizes multiple furnaces of continuous casting of such steel.

[0014] In order to achieve the above object, the present invention adopts the following technical solutions:

[0015] A method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces, comprising the following steps:

[0016] 1) heating the barrier device to 1300-1400° C. for standby use; the barrier device is a rectangular plate with a positioning hole at the center, which can float on the molten steel surface of the crystallizer and is used to block the contact between the molten steel and the protective slag;

[0017] 2) Heat the crystallizer cover plate to above 800°C and set it aside;

[0018] 3) heating and melting the low-reactivity protective slag in a graphite crucible to a liquid state, i.e. preparing a liquid protective slag for standby use;

[0019] 4) Use molybdenum wire to fix the barrier device at the bottom of the tundish, and align the positioning hole of the barrier device with the immersion nozzle; after pouring, when the continuous casting billet emerges and the molten steel liquid level is stable, cut the molybdenum wire used to fix the barrier device, so that the barrier device slowly falls to the surface of the molten steel and is sheathed on the outside of the immersion nozzle;

[0020] 5) placing the crystallizer cover plate on the top of the crystallizer, inserting the other end of the liquid slag drainage conduit led out from the graphite crucible through the crystallizer cover plate into the crystallizer, opening the valve on the liquid slag drainage conduit, and injecting liquid protective slag above the barrier device in the crystallizer;

[0021] 6) According to the slag consumption, the flow rate of the liquid protective slag is controlled by the valve on the liquid slag drainage duct until the entire casting process is completed.

[0022] Furthermore, the contact area between the barrier device and the upper surface of the molten steel accounts for 20% to 80% of the total area of ​​the upper surface of the molten steel.

[0023] Furthermore, the density of the barrier device is 4.0 g / cm 3 ~7.0g / cm 3 , thickness ≥20mm.

[0024] Furthermore, the barrier device is composed of a barrier device body and a surface spray layer; the barrier device body is made of a high-thermal-conductivity, high-temperature-resistant material; the material of the surface spray layer is one or more of high-thermal-conductivity, high-temperature-resistant, and anti-oxidation materials.

[0025] Furthermore, the high-thermal-conductivity, high-temperature-resistant material includes one or more of 2050 high-temperature alloy, titanium and corundum.

[0026] Furthermore, the material of the surface spray coating is molybdenum disilicide, hexagonal boron nitride or titanium diboride.

[0027] Furthermore, the surface spray layer is sprayed by ion spraying or laser cladding.

[0028] Furthermore, the liquid protective slag is a CaO-SiO2-based protective slag or a CaO-Al2O3-based protective slag; wherein the basicity of the CaO-SiO2-based protective slag is lower than 0.7; and the mass content of SiO2 in the CaO-Al2O3-based protective slag is ≤10%.

[0029] Furthermore, the lower surface of the crystallizer cover plate is sprayed with high-temperature radiation material.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) A barrier device is installed in the crystallizer to prevent slag-steel contact, which is used to reduce the contact area between molten steel and mold slag and inhibit the reaction ability of slag-steel. This can effectively alleviate the denaturation of mold slag and solve the problem of easy crystallization of mold slag and precipitation of slag strips;

[0032] (2) Liquid protective slag is directly added to the crystallizer equipped with a barrier device, thereby avoiding the problem of insufficient heat transfer and poor melting of solid protective slag (powder slag, granular slag, etc.) caused by the installation of a barrier device;

[0033] (3) A cover plate is added to the top of the crystallizer to solve the problem of poor thermal insulation effect of liquid protective slag;

[0034] (4) Liquid protective slag is directly added to the crystallizer to ensure the flow of protective slag into the slag channel, stabilize the slag consumption during continuous casting production, and at the same time ensure that the protective slag has stable lubrication and heat transfer functions, thus solving the problems of low slag consumption and easy bonding and steel leakage during the continuous casting of ultra-high aluminum content steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of pouring a continuous casting high-aluminum steel with ultra-high aluminum content according to the present invention.

[0036] In the figure: 1. Crystallizer 2. Immersed nozzle 3. Barrier device 4. Graphite crucible 5. Liquid slag drainage duct 6. Valve 7. Crystallizer cover 8. Molten steel 9. Solidified shell 10. Liquid protective slag DETAILED DESCRIPTION

[0037] The specific implementation of the present invention will be further described below in conjunction with the accompanying drawings:

[0038] like Figure 1 As shown, in the method for continuous casting of high-aluminum steel with ultra-high aluminum content and multiple furnaces of the present invention, a device for blocking the contact between molten steel and protective slag, namely, a blocking device 3, is adopted. The blocking device 3 is placed on the surface of the molten steel 8 of the crystallizer 1, and the contact area between the blocking device 3 and the upper surface of the molten steel 8 accounts for 20% to 80% of the total area of ​​the upper surface of the molten steel 8.

[0039] The material of the body of the barrier device 3 includes but is not limited to one or more of high thermal conductivity and high temperature resistant materials such as 2050 high temperature alloy, titanium (Ti), and corundum.

[0040] The surface of the barrier device 3 is modified by spraying one or more of high thermal conductivity, high temperature resistant and oxidation-resistant materials using ion spraying or laser cladding. The modified materials include but are not limited to molybdenum disilicide (MoSi2), hexagonal boron nitride (HBN), titanium diboride (TiB2), etc.

[0041] The density of the barrier device 3 is between 4.0 g / cm 3 ~7.0g / cm 3 It can float on the surface of molten steel and is used to block the contact between molten steel and protective slag.

[0042] A positioning hole is provided in the middle of the barrier device 3, and the horizontal movement of the barrier device 3 on the surface of the molten steel can be limited by the immersion nozzle 2. In order to ensure that the barrier device 3 has sufficient impact resistance, the thickness of the barrier device 3 is required to be ≥20mm.

[0043] A crystallizer cover plate 7 is added to the upper edge of the crystallizer 1 to play the role of heat insulation and heat preservation of the traditional protective slag with a "three-layer structure" (liquid slag layer, sintered layer, powder slag layer).

[0044] The continuous casting protection slag is melted in the graphite crucible 4 by induction heating, and the obtained liquid protection slag 10 is injected into the crystallizer 1 of the continuous casting machine through the liquid slag drainage conduit 5. The liquid protection slag 10 includes but is not limited to CaO-SiO2-based protection slag or CaO-Al2O3-based protection slag; wherein the basicity of the CaO-SiO2-based protection slag is less than 0.7; and the mass content of SiO2 in the CaO-Al2O3-based protection slag is ≤10%.

[0045] The specific operation process of the method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces is as follows:

[0046] (1) Heat the crystallizer cover plate 7 to 800° C. and heat the barrier device 3 to 1300-1400° C. for standby use.

[0047] (2) Heat and melt the protective slag in the graphite crucible 4 until it is in a liquid state and set aside.

[0048] (3) Use molybdenum wire to fix the barrier device 3 to the bottom of the tundish, and align the positioning hole in the center of the barrier device 3 with the submerged nozzle 2.

[0049] (4) The conventional continuous casting pouring process is used for the pouring operation. After the continuous casting billet emerges and the liquid level of the molten steel 8 is stable, the molybdenum wire used to fix the barrier device 3 is cut to allow the barrier device 3 to slowly fall to the surface of the molten steel 8.

[0050] (5) The crystallizer cover plate 7 is placed on the top of the crystallizer 1 , and the liquid-slag drainage conduit 5 is inserted. The other end of the liquid-slag drainage conduit 5 is connected to the graphite crucible 4 .

[0051] (5) Open the valve 6 on the liquid slag drainage conduit 5 and inject the liquid protective slag 10 above the barrier device 3 in the crystallizer 1.

[0052] (6) The flow rate of the liquid protective slag 10 is controlled according to the slag consumption. If necessary, the crystallizer cover plate 7 above the crystallizer 1 is opened to clean the slag strips that may exist in the slag channel.

[0053] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0054] [Example]

[0055] In this embodiment, a double-strand slab continuous casting machine is used to continuously cast high-aluminum steel with an Al content of 4.0wt%, a single tank of molten steel weighs 200t, the number of continuous casting tanks is 3, the cross-sectional size of the crystallizer 1 is 1100mm×230mm, and the continuous casting speed is 1.0m / min. In the double-strand slab continuous casting machine, one strand adopts a conventional casting process, and the second strand adopts the process method of the present invention.

[0056] like Figure 1 As shown, the relevant process parameters and operation procedures of the 2 streams are as follows:

[0057] 1. Make the barrier device 3; design it according to the ratio of the contact area between the barrier device 3 and the upper surface of the molten steel 8 to the total upper surface area of ​​the molten steel 8 being 65%; the barrier device 3 is a rectangular plate with a hole in the middle, with an outer size of 1000mm×170mm×30mm, and the aperture of the positioning hole at the center is During pouring, the barrier device 3 is positioned horizontally by being sleeved on the outside of the immersion nozzle 2 through the positioning hole. The frame material of the barrier device 3 is 2050 high-temperature alloy, and the interior is filled with corundum. The volume ratio of 2050 high-temperature alloy to corundum is 3:1. The outer surface of the barrier device 3 is modified by spraying molybdenum disilicide (MoSi2) powder by ion spraying. The overall density of the barrier device 3 is 7.0g / cm 3 .

[0058] 2. Make the crystallizer cover plate 7; use refractory materials to prepare the cover plate body with an outer size of 1300mm×400mm×30mm, and spray the lower surface of the cover plate body with high-temperature radiation material. Open a hole with a diameter of The circular hole is used to insert the liquid slag drainage conduits 5 on both sides. A hole with a diameter of The circular hole is used for the immersion nozzle 2 to pass through.

[0059] 3. Heat the crystallizer cover plate 7 to 800°C and the barrier device 3 to 1400°C for standby use.

[0060] 4. At a height of 500mm and a diameter of In the graphite crucible 4, the low-reactivity CaO-Al2O3-based protective slag (SiO2 mass content of 7%) is heated and melted into a liquid state for standby use.

[0061] 5. Use molybdenum wire to fix the barrier device 3 to the bottom of the tundish, and align the central positioning hole with the submerged nozzle 2.

[0062] 6. Use conventional continuous casting pouring process to carry out pouring operation. After the continuous casting billet emerges and the liquid level of molten steel 8 is stable, cut the molybdenum wire used to fix the barrier device 3, so that the barrier device 3 slowly falls to the surface of the molten steel 8 and is sleeved on the outside of the immersion nozzle 2 through the positioning hole.

[0063] 7. Place the crystallizer cover plate 7 on the top of the crystallizer 1, insert the liquid slag drainage conduit 5, and connect the other end of the liquid slag drainage conduit 5 to the graphite crucible 4.

[0064] 8. Open the valve 6 on the liquid slag drainage conduit 5 and inject liquid protective slag 10 into the crystallizer 1.

[0065] 9. Control the flow rate of liquid protective slag 10 according to the slag consumption. Open the crystallizer cover plate 7 every 30 minutes to observe whether there are slag strips in the slag channel. If there are, clean the slag strips. In the crystallizer 1, the molten steel 8 transfers heat with the water-cooled copper plate, so that the molten steel 8 solidifies into a solidified shell 9 of a certain thickness and sufficient strength. Then, under the vibration of the crystallizer 1 and the lubrication of the protective slag, the solidified shell 9 is continuously and safely pulled out of the crystallizer 1 to achieve continuous casting.

[0066] During the continuous casting process of this embodiment, the leakage prediction system of stream 1 gave 5 serious alarms within 20 minutes after the start of pouring. Only 5 kg of protective slag was consumed during the pouring process, and a large number of slag strips appeared on the liquid surface of the crystallizer. The pouring was forced to stop after 20 minutes. However, the leakage prediction system of stream 2 did not give any alarm during the entire pouring process, and successfully completed the multi-furnace continuous casting of 3 tanks of high-aluminum steel.

[0067] From the above comparison, it can be seen that the method for continuous casting of high-aluminum steel with ultra-high aluminum content and multiple furnaces of the present invention can realize multiple furnaces of continuous casting of such steel, thus ensuring the smooth continuous casting production.

[0068] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces, characterized in that: The steps include: 1) heating the barrier device to 1300-1400° C. for standby use; the barrier device is a rectangular plate with a positioning hole at the center, which can float on the molten steel surface of the crystallizer and is used to block the contact between the molten steel and the protective slag; 2) Heat the crystallizer cover plate to above 800°C and set aside; 3) heating and melting the low-reactivity protective slag in a graphite crucible to a liquid state, i.e. preparing a liquid protective slag for standby use; 4) Use molybdenum wire to fix the barrier device at the bottom of the tundish, and align the positioning hole of the barrier device with the immersion nozzle; after pouring, when the continuous casting billet emerges and the molten steel liquid level is stable, cut the molybdenum wire used to fix the barrier device, so that the barrier device slowly falls to the surface of the molten steel and is sheathed on the outside of the immersion nozzle; 5) placing the crystallizer cover plate on the top of the crystallizer, inserting the other end of the liquid slag drainage conduit led out from the graphite crucible through the crystallizer cover plate into the crystallizer, opening the valve on the liquid slag drainage conduit, and injecting liquid protective slag above the barrier device in the crystallizer; 6) According to the slag consumption, the flow rate of the liquid protective slag is controlled by the valve on the liquid slag drainage duct until the entire casting process is completed.

2. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 1 is characterized in that: The contact area between the barrier device and the upper surface of the molten steel accounts for 20% to 80% of the total area of ​​the upper surface of the molten steel.

3. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 1 is characterized in that: The density of the barrier device is 4.0 g / cm 3 ~7.0g / cm 3 , thickness ≥20mm.

4. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 1, 2 or 3, characterized in that: The barrier device is composed of a barrier device body and a surface spray layer; the barrier device body is made of a high-thermal-conductivity, high-temperature-resistant material; the material of the surface spray layer is one or more of high-thermal-conductivity, high-temperature-resistant, and anti-oxidation materials.

5. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 4, characterized in that: The high-thermal-conductivity, high-temperature-resistant material includes one or more of high-temperature alloy, titanium and corundum.

6. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 4, characterized in that: The material of the surface spray coating is molybdenum disilicide, hexagonal boron nitride or titanium diboride.

7. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 4, characterized in that: The surface spray layer is sprayed by ion spraying or laser cladding.

8. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 1, characterized in that: The liquid protective slag is a CaO-SiO2-based protective slag or a CaO-Al2O3-based protective slag; wherein the basicity of the CaO-SiO2-based protective slag is lower than 0.7; and the mass content of SiO2 in the CaO-Al2O3-based protective slag is ≤10%.

9. The method for continuous casting of ultra-high aluminum content high aluminum steel with multiple furnaces according to claim 1, characterized in that: The lower surface of the crystallizer cover plate is sprayed with high-temperature radiation material.

Citation Information

Patent Citations

  • Mold flux and casting method using same

    CN109070201A

  • Jig for casting and casting method using same

    CN109562443A

  • Isolating plate structure for continuous casting of molten steel

    CN112296286A

  • Pour into a mould crystallizer apron device that liquid covering slag was used

    CN205732868U

  • Device and Method for preventing the Growth of SlagBear in the Mold for Continuous Casting of Steel

    KR1020020052622A

Cited By

  • Device and method for preparing large cast ingot through layer-by-layer solidification