Method for improving hardness of 316L stainless steel

By adding iron-based amorphous powder to the LPBF process and performing laser powder bed fusion, the problem of low hardness and cracks in 316L stainless steel is solved, the hardness is improved and performance is optimized, and meets higher usage requirements.

CN118720127APending Publication Date: 2024-10-01KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411114195.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The hardness of 316L stainless steel prepared by LPBF process is low, and due to poor wettability between metal and ceramics, it is easy to cause cracks and affect the performance of components.

Method used

Iron-based amorphous powder is added to 316L stainless steel and formed through laser powder bed fusion technology. The good wettability and high strength of iron-based amorphous and 316L stainless steel make it evenly dispersed, increasing hardness and reducing the probability of cracks.

Benefits of technology

Significantly improves the hardness and performance of 316L stainless steel, reduces cracks during the manufacturing process, and enhances the overall hardness and wear resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720127A_ABST
    Figure CN118720127A_ABST
Patent Text Reader

Abstract

The invention discloses a method for improving the hardness of 316L stainless steel, and belongs to the technical field of additive manufacturing metal materials. The method comprises the following steps: (1) uniformly mixing iron-based amorphous powder and 316L stainless steel powder, and carrying out vacuum drying to obtain mixed powder; and (2) the mixed powder obtained in the step (1) is formed in a laser powder bed melting mode, and the stainless steel component is obtained. According to the method, in the process of manufacturing the 316L stainless steel through the LPBF, the iron-based amorphous is added to strengthen the stainless steel, and meanwhile, cracks are reduced, so that the 316L stainless steel component which is high in density, low in porosity and high in hardness is prepared, and the use performance of the 316L stainless steel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of additive manufacturing metal materials and relates to a method for improving the hardness of 316L stainless steel. Background Art

[0002] Laser Powder Bed Fusion (LPBF), also known as Selective Laser Melting (SLM) technology, has been developed for nearly 40 years since its birth. With the development of computer control technology and laser technology, this technology has become more and more mature in recent years. Its processing principle is to first generate a computer-aided design (CAD) model of the completed component. Then the model is divided into several layers (that is, the three-dimensional model is sliced ​​to obtain two-dimensional slices, and the file is saved in STL format and imported into the computer-aided system of the laser powder bed melting equipment). The pre-deposited metal powder is evenly distributed to each layer, and the laser beam accurately melts the metal powder in the specified area controlled by the computer. Subsequently, the process of melting and depositing powder is performed layer by layer, and finally a metal layer with a cross-section similar to that of a specific part of the part is formed. The above process is repeated until the metal component is consistent with the CAD model. Due to this feature, this technology can be used to directly process some complex-shaped parts. The production of mechanical parts is almost not restricted by geometric shapes, and does not require many expensive processing tools. It has the advantages of high design freedom, short part molding cycle, high molding accuracy, and high material utilization.

[0003] 316L stainless steel is a low-carbon austenitic stainless steel containing 16.5-18.5% chromium by mass and a small amount of alloying elements such as nickel, molybdenum, and manganese. It has good high-temperature tensile properties and creep strength, corrosion resistance, and radiation damage resistance. It is used in the primary side of liquid metal cooled fast neutron breeder reactors (LMFBRs) and in ships, biomedical equipment, and fuel cells. It is currently one of the most widely used stainless steel materials. However, the traditional manufacturing process of 316L stainless steel components is quite complicated, and the cost is high and the economy is poor. For example, when manufacturing 316L stainless steel components by casting, subsequent machining and other treatments are generally required, the process is complicated, the production cycle is long, and it is not easy to form 316L stainless steel parts with complex shapes. In order to meet the needs of diverse applications, higher requirements are also put forward for the performance of 316L stainless steel and component manufacturing technology.

[0004] 316L stainless steel components prepared by LPBF process can overcome the problems existing in traditional manufacturing processes. However, during the LPBF process, due to the high cooling rate, the microstructure of 316L stainless steel will form an uneven structure, including fine grains and substructures. Although fine grains will play a certain strengthening role in the hardness of 316L stainless steel, due to its uneven structure, it has a certain negative impact on the hardness of 316L stainless steel. Therefore, there is still a lot of room for improvement in the hardness of 316L stainless steel prepared by LPBF process. At the same time, 316L stainless steel itself is an austenitic stainless steel, mainly existing in austenite phase. The austenite phase is usually lower in hardness than the ferrite or martensite phase, which also leads to the problem of low hardness even if 316L stainless steel is prepared by LPBF process. In order to improve the hardness of 316L stainless steel manufactured by LPBF, at present, ceramics are mostly added as a reinforcing phase to strengthen the stainless steel matrix. However, due to the poor wettability between metal and ceramic, cracks are easily generated during the manufacturing process of 316L stainless steel, resulting in a decrease in its strength and a great impact on the performance of the component.

[0005] Therefore, it is necessary to provide a method for improving the hardness of 316L stainless steel, to improve the hardness of 316L stainless steel manufactured by LPBF process, and thus to improve the performance of 316L stainless steel. Summary of the invention

[0006] In order to overcome the problems in the background technology, the present invention uses iron-based amorphous to strengthen 316L stainless steel. The iron-based amorphous has good wettability with 316L stainless steel. When added as a reinforcing phase, the probability of cracks in the manufacturing process of 316L stainless steel can be effectively reduced during the manufacturing process of the component. At the same time, on the one hand, the iron-based amorphous itself has high strength. It is evenly dispersed in 316L stainless steel and tightly combined with 316L stainless steel, which can more evenly improve the strength of each point of 316L stainless steel; on the other hand, the iron-based amorphous also micro-strengthens 316L stainless steel to further improve the hardness of 316L stainless steel on the basis of reducing the elongation of 316L stainless steel.

[0007] In order to achieve the above object, the present invention is implemented by the following scheme:

[0008] The method comprises the following steps:

[0009] (1) uniformly mixing iron-based amorphous powder and 316L stainless steel powder and vacuum drying to obtain a mixed powder;

[0010] (2) The mixed powder obtained in step (1) is molded by laser powder bed melting to obtain a stainless steel component.

[0011] Preferably, in the mixed powder in step (1), the iron-based amorphous powder accounts for 0.2 to 1.0 wt % of the total mass of the mixed powder.

[0012] Preferably, the iron-based amorphous powder is Fe 95.7 C 0.5 B 3.8 powder.

[0013] Preferably, the iron-based amorphous powder has a particle size of 0 to 15 μm.

[0014] Preferably, the particle size of the 316L stainless steel powder is 15-53 μm.

[0015] Preferably, in step (1), the drying temperature is 80° C. and the drying time is 4 to 6 hours.

[0016] Preferably, in the step (1), the iron-based amorphous powder and the 316L stainless steel powder are evenly mixed by ball milling. During the ball milling mixing process, argon gas is introduced into the ball mill for protection. The ball milling time is 3 to 5 hours, the ball milling speed is 60 to 150 r / min, and the ball mill is paused for 20 minutes after each 20-minute rotation.

[0017] Preferably, in the step (2), the specific method of laser powder bed melting is: laying a layer of mixed powder on the forming substrate of the laser powder bed melting equipment, and the fiber laser of the laser powder bed melting equipment melts the mixed powder according to a preset program. After each layer of mixed powder is processed, the forming substrate is lowered by 20 to 40 μm, and a new layer of mixed powder is laid on it for processing, and the mixed powder laying and laser processing process are repeated until the entire component is processed.

[0018] Preferably, during the laser powder bed melting process, the laser power is 75-95 W, the laser scanning speed is 1000-1400 mm / s, the scanning spacing is 60 μm, the scanning strategy is S-type orthogonal, the interlayer angle is set to 67°, and each layer of mixed powder is melted 1 to 2 times.

[0019] Preferably, the composition of the 316L stainless steel powder is as follows by mass percentage: Cr: 17-19%, Ni: 10-14%, Mo: 2-3%, Mn: ≤2%, C: ≤0.03%, Si: ≤0.75%, P: ≤0.05%, S: ≤0.03%, N: ≤0.1%, and the balance is Fe.

[0020] Beneficial effects of the present invention:

[0021] 1. The present invention increases the hardness of 316L stainless steel by adding iron-based amorphous during the process of manufacturing 316L stainless steel using LPBF, while reducing cracks generated during the manufacturing process, so that the component has more excellent performance.

[0022] 2. During the LPBF forming process, the cooling rate can reach 106K / s, which is greater than the formation condition of iron-based amorphous 103K / s. In the LPBF process of manufacturing 316L stainless steel, adding iron-based amorphous powder can form an iron-based amorphous structure more stably.

[0023] 3. The present invention uses Fe 95.7 C 0.5 B 3.8 Powder, using the characteristics of boron having a higher growth restriction factor in iron-based materials, boron solute providing a higher component supercooling, and boron being able to refine the epitaxial grains in 316L stainless steel, the boron element interacts with 316L stainless steel, so that after the 316L stainless steel solidifies, its honeycomb and grain size are significantly reduced; thereby achieving the purpose of improving the hardness of 316L stainless steel.

[0024] 4. Boride is a hard phase, using Fe 95.7 C 0.5 B 3.8 Powder helps to improve the overall hardness and wear resistance of the material.

[0025] 5. The present invention uses Fe 95.7 C 0.5 B 3.8 Powder causes carbides to precipitate at grain boundaries and hinder dislocation movement, thereby increasing the hardness of the material. At a certain concentration, carbon can stabilize the austenite phase and improve its strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the element energy spectrum distribution diagram of the iron-based amorphous powder in Example 1 of the present invention;

[0027] Figure 2 The metallographic images of the stainless steel samples prepared in the embodiments and comparative examples of the present invention are shown in Figure (a) as the metallographic image of the stainless steel sample of comparative example 1, Figure (b) as the metallographic image of the stainless steel sample of embodiment 1, Figure (c) as the metallographic image of the stainless steel sample of embodiment 2, Figure (d) as the metallographic image of the stainless steel sample of embodiment 3, Figure (e) as the metallographic image of the stainless steel sample of embodiment 4, and Figure (f) as the metallographic image of the stainless steel sample of embodiment 5;

[0028] Figure 3The microstructure diagrams of the stainless steel samples prepared in the embodiments and comparative examples of the present invention, wherein (a) is the microstructure diagram of the stainless steel sample of comparative example 1, wherein (b) is the microstructure diagram of the stainless steel sample of embodiment 1, wherein (c) is the microstructure diagram of the stainless steel sample of embodiment 3, wherein (d) is the microstructure diagram of the stainless steel sample of embodiment 4;

[0029] Figure 4 XRD diagram of stainless steel samples prepared in the embodiments and comparative examples of the present invention;

[0030] Figure 5 The microhardness diagram of stainless steel samples prepared in the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with specific embodiments.

[0032] In the examples and comparative examples of the present invention, chemical reagents not specifically described were used in the experiments using commercially available analytically pure reagents.

[0033] Example 1

[0034] In this example, the stainless steel sample was prepared by the following method:

[0035] (1) Use 400 mesh, 800 mesh and 1500 mesh sieves to screen out Fe particles with a particle size of 0 to 15 μm. 95.7 C 0.5 B 3.8 and 316L stainless steel powder with a particle size of 15 to 53 μm. The composition of the 316L stainless steel powder is as follows by mass percentage: Cr: 17 to 19%, Ni: 10 to 14%, Mo: 2 to 3%, Mn: ≤2%, C: ≤0.03%, Si: ≤0.75%, P: ≤0.05%, S: ≤0.03%, N: ≤0.1%, and the balance is Fe.

[0036] (2) The screened Fe 95.7 C 0.5 B 3.8 The powder and stainless steel powder are mixed in a mass ratio of 2:98, and then the prepared powder is added into a ball mill for mechanical mixing to obtain a mixed powder. Argon gas is introduced into the ball mill for protection. The ball milling time is 4 hours and the speed is 150r / min. The ball mill rotates for 20 minutes and pauses for 20 minutes for cooling. The ball-to-material ratio is matched in a ratio of 4:1.

[0037] (3) The mixed powder is placed in a vacuum dryer for drying; the dryer is evacuated to a vacuum state, the drying time is 5 hours, and the drying temperature is 80° C.; the mixed powder is allowed to cool to room temperature under vacuum.

[0038] (4) 3D modeling was performed using 3DMax software, and the 3D model was imported into a slicing software for slicing with a slice thickness of 20 μm. After processing, the slicing was saved as an STL file, and the STL file was imported into the LPBF device.

[0039] (5) The substrate used for molding is cleaned with alcohol and then blown dry, and the stainless steel substrate is installed in the molding chamber of the LPBF equipment; the dried mixed powder is added to the powder bin of the LPBF equipment, and argon gas is introduced into the molding chamber to keep the oxygen content in the molding chamber less than 500 ppm.

[0040] (6) A scraper is used to spread a layer of mixed powder on the molded substrate, and a fiber laser is used to melt the powder according to the geometric shape of the two-dimensional slice. The laser scanning process parameters are: laser power of 85 W, laser scanning speed of 1000 mm / s, and laser scanning interval of 60 μm.

[0041] (7) After each layer is processed, the substrate is lowered 20 μm and a new layer of powder is applied. This cycle is repeated until a stainless steel sample is processed.

[0042] Example 2

[0043] In this example, the stainless steel sample was prepared by the following method:

[0044] (1) Use 400 mesh, 800 mesh and 1500 mesh sieves to screen out Fe particles with a particle size of 0 to 15 μm. 95.7 C 0.5 B 3.8 and 316L stainless steel powder with a particle size of 15 to 53 μm. The composition of the 316L stainless steel powder is as follows by mass percentage: Cr: 17 to 19%, Ni: 10 to 14%, Mo: 2 to 3%, Mn: ≤2%, C: ≤0.03%, Si: ≤0.75%, P: ≤0.05%, S: ≤0.03%, N: ≤0.1%, and the balance is Fe.

[0045] (2) The screened Fe 95.7 C 0.5 B 3.8 The powder and stainless steel powder are mixed in a mass ratio of 4:96, and then the prepared powder is added into a ball mill for mechanical mixing to obtain a mixed powder. Argon gas is introduced into the ball mill for protection. The ball milling time is 3 hours and the speed is 150r / min. The ball mill rotates for 20 minutes and pauses for 20 minutes for cooling. The ball-to-material ratio is matched in a ratio of 4:1.

[0046] (3) The mixed powder is placed in a vacuum dryer for drying; the dryer is evacuated to a vacuum state, the drying time is 4 hours, and the drying temperature is 80° C.; the mixed powder is allowed to cool to room temperature under vacuum.

[0047] (4) 3D modeling was performed using 3DMax software, and the 3D model was imported into a slicing software for slicing with a slice thickness of 40 μm. After processing, the slicing was saved as an STL file, and the STL file was imported into the LPBF device.

[0048] (5) The substrate used for molding is cleaned with alcohol and then blown dry, and the stainless steel substrate is installed in the molding chamber of the LPBF equipment; the dried mixed powder is added to the powder bin of the LPBF equipment, and argon gas is introduced into the molding chamber to keep the oxygen content in the molding chamber less than 500 ppm.

[0049] (6) A scraper is used to spread a layer of mixed powder on the molded substrate, and a fiber laser is used to melt the powder according to the geometric shape of the two-dimensional slice. The laser scanning process parameters are: laser power of 75 W, laser scanning speed of 1000 mm / s, and laser scanning spacing of 60 μm.

[0050] (7) After each layer is processed, the substrate is lowered 40 μm and a new layer of powder is applied. This cycle is repeated until a stainless steel sample is processed.

[0051] Example 3

[0052] In this example, the stainless steel sample was prepared by the following method:

[0053] (1) Use 400 mesh, 800 mesh and 1500 mesh sieves to screen out Fe particles with a particle size of 0 to 15 μm. 95.7 C 0.5 B 3.8 and 316L stainless steel powder with a particle size of 15 to 53 μm. The composition of the 316L stainless steel powder is as follows by mass percentage: Cr: 17 to 19%, Ni: 10 to 14%, Mo: 2 to 3%, Mn: ≤2%, C: ≤0.03%, Si: ≤0.75%, P: ≤0.05%, S: ≤0.03%, N: ≤0.1%, and the balance is Fe.

[0054] (2) The screened Fe 95.7 C 0.5 B 3.8 The powder and stainless steel powder are mixed in a mass ratio of 6:94, and then the prepared powder is added into a ball mill for mechanical mixing to obtain a mixed powder. Argon gas is introduced into the ball mill for protection. The ball milling time is 5 hours and the speed is 60r / min. The ball mill rotates for 20 minutes and pauses for 20 minutes for cooling. The ball-to-material ratio is matched in a ratio of 4:1.

[0055] (3) The mixed powder is placed in a vacuum dryer for drying; the dryer is evacuated to a vacuum state, the drying time is 6 hours, and the drying temperature is 80° C.; the mixed powder is allowed to cool to room temperature under vacuum.

[0056] (4) 3D modeling was performed using 3DMax software, and the 3D model was imported into a slicing software for slicing with a slice thickness of 30 μm. After processing, the slicing was saved as an STL file, and the STL file was imported into the LPBF device.

[0057] (5) The substrate used for molding is cleaned with alcohol and then blown dry, and the stainless steel substrate is installed in the molding chamber of the LPBF equipment; the dried mixed powder is added to the powder bin of the LPBF equipment, and argon gas is introduced into the molding chamber to keep the oxygen content in the molding chamber less than 500 ppm.

[0058] (6) A scraper is used to spread a layer of mixed powder on the molded substrate, and a fiber laser is used to melt the powder according to the geometric shape of the two-dimensional slice. The laser scanning process parameters are: laser power of 95 W, laser scanning speed of 1400 mm / s, and laser scanning spacing of 60 μm.

[0059] (7) After each layer is processed, the substrate is lowered by 30 μm and a new layer of powder is applied. This cycle is repeated until a stainless steel sample is processed.

[0060] Example 4

[0061] In this example, the stainless steel sample was prepared by the following method:

[0062] (1) Use 400 mesh, 800 mesh and 1500 mesh sieves to screen out Fe particles with a particle size of 0 to 15 μm. 95.7 C 0.5 B 3.8 and 316L stainless steel powder with a particle size of 15 to 53 μm. The composition of the 316L stainless steel powder is as follows by mass percentage: Cr: 17 to 19%, Ni: 10 to 14%, Mo: 2 to 3%, Mn: ≤2%, C: ≤0.03%, Si: ≤0.75%, P: ≤0.05%, S: ≤0.03%, N: ≤0.1%, and the balance is Fe.

[0063] (2) The screened Fe 95.7 C 0.5 B 3.8 The powder and stainless steel powder are mixed in a mass ratio of 8:92, and then the prepared powder is added into a ball mill for mechanical mixing to obtain a mixed powder. Argon gas is introduced into the ball mill for protection. The ball milling time is 4 hours and the speed is 100r / min. The ball mill rotates for 20 minutes and pauses for 20 minutes for cooling. The ball-to-material ratio is matched in a ratio of 4:1.

[0064] (3) The mixed powder is placed in a vacuum dryer for drying; the dryer is evacuated to a vacuum state, the drying time is 5 hours, and the drying temperature is 80° C.; the mixed powder is allowed to cool to room temperature under vacuum.

[0065] (4) 3D modeling was performed using 3DMax software, and the 3D model was imported into a slicing software for slicing with a slice thickness of 20 μm. After processing, the slicing was saved as an STL file, and the STL file was imported into the LPBF device.

[0066] (5) The substrate used for molding is cleaned with alcohol and then blown dry, and the stainless steel substrate is installed in the molding chamber of the LPBF equipment; the dried mixed powder is added to the powder bin of the LPBF equipment, and argon gas is introduced into the molding chamber to keep the oxygen content in the molding chamber less than 500 ppm.

[0067] (6) A scraper is used to spread a layer of mixed powder on the molded substrate, and a fiber laser is used to melt the powder according to the geometric shape of the two-dimensional slice. The laser scanning process parameters are: laser power of 85 W, laser scanning speed of 1200 mm / s, and laser scanning interval of 60 μm.

[0068] (7) After each layer is processed, the substrate is lowered 20 μm and a new layer of powder is applied. This cycle is repeated until a stainless steel sample is processed.

[0069] Example 5

[0070] In this example, the stainless steel sample was prepared by the following method:

[0071] (1) Use 400 mesh, 800 mesh and 1500 mesh sieves to screen out Fe particles with a particle size of 0 to 15 μm. 95.7 C 0.5 B 3.8 and 316L stainless steel powder with a particle size of 15 to 53 μm. The composition of the 316L stainless steel powder is as follows by mass percentage: Cr: 17 to 19%, Ni: 10 to 14%, Mo: 2 to 3%, Mn: ≤2%, C: ≤0.03%, Si: ≤0.75%, P: ≤0.05%, S: ≤0.03%, N: ≤0.1%, and the balance is Fe.

[0072] (2) The screened Fe 95.7 C 0.5 B 3.8 The powder and stainless steel powder are mixed in a mass ratio of 10:90, and then the prepared powder is added into a ball mill for mechanical mixing to obtain a mixed powder. Argon gas is introduced into the ball mill for protection. The ball milling time is 4 hours and the speed is 150r / min. The ball mill rotates for 20 minutes and pauses for 20 minutes for cooling. The ball-to-material ratio is matched in a ratio of 4:1.

[0073] (3) The mixed powder is placed in a vacuum dryer for drying; the dryer is evacuated to a vacuum state, the drying time is 5 hours, and the drying temperature is 80° C.; the mixed powder is allowed to cool to room temperature under vacuum.

[0074] (4) 3D modeling was performed using 3DMax software, and the 3D model was imported into a slicing software for slicing with a slice thickness of 20 μm. After processing, the slicing was saved as an STL file, and the STL file was imported into the LPBF device.

[0075] (5) The substrate used for molding is cleaned with alcohol and then blown dry, and the stainless steel substrate is installed in the molding chamber of the LPBF equipment; the dried mixed powder is added to the powder bin of the LPBF equipment, and argon gas is introduced into the molding chamber to keep the oxygen content in the molding chamber less than 500 ppm.

[0076] (6) A scraper is used to spread a layer of mixed powder on the molded substrate, and a fiber laser is used to melt the powder according to the geometric shape of the two-dimensional slice. The laser scanning process parameters are: laser power of 85 W, laser scanning speed of 1000 mm / s, and laser scanning interval of 60 μm.

[0077] (7) After each layer is processed, the substrate is lowered 20 μm and a new layer of powder is applied. This cycle is repeated until a stainless steel sample is processed.

[0078] Comparative Example 1

[0079] The method for preparing the 316L stainless steel sample in this comparative example is the same as that in Example 1, except that: no iron-based amorphous powder is added in this comparative example.

[0080] Comparative Example 2

[0081] The method for preparing 316L stainless steel sample in this comparative example is the same as that in Example 1, except that the iron-based amorphous powder added in this comparative example is FeCoCrMoCBY. Although the strength of the stainless steel sample in this comparative example is improved, the elongation drops sharply from 24% to 9.8%. 95.7 C 0.5 B 3.8 As an iron-based amorphous powder, the carbon content is relatively low, but the carbon content of the present invention is sufficient to form carbides such as Fe3C, which are evenly distributed in the matrix to provide a strengthening effect, and excessive carbon will cause a large amount of carbides to form. Although it can greatly improve the hardness and strength of the material, excessive carbides will cause the material to become brittle, thereby affecting the toughness and machinability of the material. Therefore, controlling the carbon content to a specific value can achieve the purpose of significantly improving the hardness and strength of the material without affecting the toughness and machinability of the material too much. Boron in the iron-based amorphous powder can also form hard borides such as Fe2B. A low boron content will make the strengthening effect of the iron-based amorphous powder poor, and an excessive boron content will also increase the brittleness of the material, which is not conducive to material processing.

[0082] pass Figure 1It can be seen that through powder mixing, the small-particle iron-based amorphous powder and the 316L powder are evenly mixed.

[0083] pass Figure 2 It can be seen that the unique fish-scale-like melt pool of the sample prepared by SLM with a chessboard scanning trajectory, Figure 2 Compared with the unreinforced stainless steel samples, the stainless steel samples of the present invention have no macroscopic defects, indicating that particle-particle metallurgical bonding occurs when the composite powder is almost completely melted, and no defects are generated during the preparation of 316L stainless steel samples of the present invention. At the same time, the printed samples contain mainly columnar grains, which grow in the molten pool. However, these columnar grains are confined to a single weld or multiple layers, which indicates that new grains grow along the direction of the maximum temperature gradient in the remelting zone.

[0084] pass Figure 3 It can be seen that epitaxial grains are clearly visible in the microstructure of the 316L stainless steel sample. When the iron-based amorphous powder of the present invention is added, epitaxial grains can also be observed in the printed part. However, when more iron-based amorphous powder is added, the epitaxial grains become almost invisible in the printed part, indicating that the added iron-based amorphous powder of the present invention can prevent the epitaxy of the grains.

[0085] pass Figure 4 It can be seen that the γ phase (austenite, marked as a star) and α phase (ferrite, marked as a rhombus) appear in the diffraction peaks of all stainless steel samples, which is a typical Fe matrix structural feature. Since Fe is the main component of 316L stainless steel, it also plays a role in solid solution strengthening in the iron-based amorphous powder of the present invention, and further improves the mechanical properties of the material by forming a solid solution in the 316L stainless steel matrix. As the amount of iron-based amorphous powder added increases, the peaks of the γ phase and the α phase gradually weaken, indicating that the amount of iron-based amorphous powder added has a significant effect on the matrix structure, and the amount of iron-based amorphous powder added needs to be controlled to form a good synergistic effect, so that the 316L stainless steel matrix can obtain an excellent strengthening effect.

[0086] pass Figure 5 It can be seen that the present invention can significantly improve the hardness of 316L stainless steel by adding iron-based amorphous into 316L stainless steel. Compared with comparative example 1, when the addition amount of iron-based amorphous is 1wt%, the hardness of the stainless steel is increased by 167.08HV, and the hardness can reach about 450HV.

[0087] In summary, the present invention can significantly improve the hardness of 316L stainless steel and effectively reduce or avoid the generation of cracks by adding iron-based amorphous powder in the process of LPBF manufacturing 316L stainless steel, thereby obtaining 316L stainless steel with excellent performance and meeting the use requirements of 316L stainless steel in a wider range.

[0088] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A method for improving the hardness of 316L stainless steel, Features: The method comprises the following steps: (1) uniformly mixing iron-based amorphous powder and 316L stainless steel powder and vacuum drying to obtain a mixed powder; (2) The mixed powder obtained in step (1) is molded by laser powder bed melting to obtain a stainless steel component.

2. A method for improving the hardness of 316L stainless steel according to claim 1, Features: In the mixed powder in step (1), the iron-based amorphous powder accounts for 0.2 to 1.0 wt % of the total mass of the mixed powder.

3. A method for improving the hardness of 316L stainless steel according to claim 1, Features: The iron-based amorphous powder is Fe 95.7 C 0.5 B 3.8 powder.

4. A method for improving the hardness of 316L stainless steel according to claim 1, Features: The particle size of the iron-based amorphous powder is 0 to 15 μm.

5. A method for improving the hardness of 316L stainless steel according to claim 1, Features: The particle size of the 316L stainless steel powder is 15-53 μm.

6. A method for improving the hardness of 316L stainless steel according to claim 1, Features: In the step (1), the drying temperature is 80° C. and the drying time is 4 to 6 hours.

7. A method for improving the hardness of 316L stainless steel according to claim 1, Features: In the step (1), the iron-based amorphous powder and the 316L stainless steel powder are evenly mixed by ball milling. During the ball milling, argon gas is introduced into the ball mill for protection. The ball milling time is 3 to 5 hours, the ball milling speed is 60 to 150 r / min, and the ball mill is paused for 20 minutes after each 20-minute rotation.

8. A method for improving the hardness of 316L stainless steel according to claim 1, Features: In the step (2), the specific method of laser powder bed melting is: laying a layer of mixed powder on the forming substrate of the laser powder bed melting equipment, and the fiber laser of the laser powder bed melting equipment melts the mixed powder according to a preset program. After each layer of mixed powder is processed, the forming substrate is lowered by 20 to 40 μm, and a new layer of mixed powder is laid on it for processing. The mixed powder laying and laser processing process are repeated until the entire component is processed.

9. A method for improving the hardness of 316L stainless steel according to claim 8, Features: During the laser powder bed melting process, the laser power is 75-95W, the laser scanning speed is 1000-1400mm / s, the scanning spacing is 60μm, the scanning strategy is S-type orthogonal, the interlayer rotation angle is set to 67°, and each layer of mixed powder is melted 1-2 times.

10. A method for improving the hardness of 316L stainless steel according to any one of claims 1 to 9, Features: The composition of the 316L stainless steel powder is as follows by mass percentage: Cr: 17-19%, Ni: 10-14%, Mo: 2-3%, Mn: ≤2%, C: ≤0.03%, Si: ≤0.75%, P: ≤0.05%, S: ≤0.03%, N: ≤0.1%, and the balance is Fe.

Citation Information

Cited By

  • High-strength bolt and preparation method thereof

    CN119287271A