Method for producing welded structure and welding device

By using the stack welding method in the welding structure and controlling the size and time period of the current, the problem of burr formation when the distance between welding points becomes shorter is solved and the welding quality is improved.

CN118720375APending Publication Date: 2024-10-01TOYOTA JIDOSHA KK +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410318133.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-20
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing welding technology easily forms burrs when the distance between welding points becomes shorter, resulting in a decrease in welding quality.

Method used

By using a stacked welding method in the welding structure, the size and time period of the current are controlled to ensure that the time period when the main current flows through the welding point is longer than the time period when the large current flows through the welding point, and the current is adjusted when the welding point is pressurized. Conversion from large current to main current reduces the formation of burrs.

Benefits of technology

It effectively reduces the formation of burrs at welding points and improves welding quality, especially when the distance between welding points is short.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720375A_ABST
    Figure CN118720375A_ABST
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a welded structure and a welding device. Provided are a method for manufacturing a welded structure and a welding apparatus capable of reducing burr formation. The method for manufacturing a welded structure according to the present disclosure is a method for manufacturing a welded structure formed by spot welding a laminate formed of three or more metal plates, at least one metal plate among the three or more metal plates being thinner than the other metal plates. The manufacturing method includes a step of energizing a welding point of the laminated body while pressurizing the welding point and causing a main current to flow through the welding point of the laminated body, and a step of continuously energizing the welding point of the laminated body while pressurizing the welding point and causing a large current larger than the main current to flow through the welding point of the laminated body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing a welded structure and a welding device. Background Art

[0002] Japanese Patent No. 7038193 discloses a spot welding method for joining a laminated body formed by laminating three or more metal plates on each other, at least one of which is formed to have a thickness different from that of the other metal plates, using a pulse current. Summary of the invention

[0003] The applicant has found the following problems.

[0004] When the distance between the welded welding point and the welding point to be welded becomes shorter, the burr may be formed. For example, when a welding point positioned between the welded welding points that have already been welded is energized while it is pressurized, the current may be transferred to the welded welding point, and the burr may be formed at the energized welding point. When, for example, molten metal generated just below the welding point when energization is applied is ejected from the surface of the welding point and hardened, the burr is formed.

[0005] The present disclosure has been made in view of the above problems, and proposes a method for manufacturing a welded structure and a welding device, which are capable of reducing the formation of burrs.

[0006] The method for manufacturing a welded structure according to the present disclosure is a method for manufacturing a welded structure formed by spot welding a laminated body formed of three or more metal plates laminated on each other, at least one of the three or more metal plates being thinner than the other metal plates, the method comprising: energizing the welded points of the laminated body while pressurizing the welded points and causing a main current to flow through the welded points of the laminated body; and continuously energizing the welded points of the laminated body while pressurizing the welded points and causing a large current greater than the main current to flow through the welded points of the laminated body, wherein a time period t for causing the main current to flow through the welded points of the laminated body is 1 longer than the time period t for causing the large current to flow through the welding point of the stacked body. 2 .

[0007] Furthermore, in the above method for manufacturing a welded structure, the time period t during which the main current flows through the weld point of the stacked body is 1 It can be the time period t during which a large current flows through the welding point of the laminated body. 2 2.50 times or more.

[0008] Further, in the above-mentioned method for manufacturing a welded structure, the current value A2 of the large current may be 12 kA or more.

[0009] A method for manufacturing a welding structure according to the present disclosure is a method for manufacturing the following welding structure, which is formed by spot welding a stacked body formed by three or more metal plates stacked on each other, at least one of the three or more metal plates is thinner than the other metal plates, and the method includes: energizing the welding points of the stacked body while pressurizing them and causing a matching current to flow through the welding points of the stacked body; continuously energizing the welding points of the stacked body while pressurizing them and causing a large current to flow through the welding points of the stacked body; and continuously energizing the welding points of the stacked body while pressurizing them and causing a main current smaller than the large current to flow through the welding points of the stacked body, wherein a current value A13 of the matching current is smaller than a current value A11 of the main current.

[0010] Furthermore, in the above method for manufacturing a welded structure, the time period t for which the main current is made to flow through the weld point of the stacked body is 11 The time period t during which the high current flows through the welding point of the stacked body may be 12 2.50 times or more.

[0011] Furthermore, in the above method for manufacturing a welded structure, the time period t for which the main current is made to flow through the weld point of the stacked body is 11 The time period t during which the matching current flows through the welding point of the stack may be 13 3.00 times or less of.

[0012] Furthermore, in the above-described method for manufacturing a welded structure, the current value A13 of the matching current may be 0.95 times or less the current value A11 of the main current.

[0013] Further, in the above method for manufacturing a welded structure, the stacked body may include welded points that have been welded, and the welded points of the stacked body are within 15 mm from the welded points.

[0014] The method for manufacturing a welded structure according to the present disclosure is a method for manufacturing a welded structure formed by spot welding a laminated body formed of three or more metal plates laminated on each other, at least one of the three or more metal plates being thinner than the other metal plates, the method comprising: determining a method for welding the welded points to be welded based on the positions of the welded points to be welded, wherein, in the determination of the welding method, when the distance between the welded points to be welded and the welded points that have been welded exceeds a predetermined value, energizing the welded points of the laminated body while they are pressurized and causing a large current to flow through the welded points of the laminated body , then the welding point of the laminated body is continuously energized while it is pressurized and a main current smaller than the large current is passed through the welding point of the laminated body, and when the distance between the welding point to be welded and the welded welding point is a predetermined value or less, the welding point to be welded is welded using a welding method in which the welding point of the laminated body is energized while it is pressurized and the main current is passed through the welding point of the laminated body, and then the welding point of the laminated body is continuously energized while it is pressurized and a large current larger than the main current is passed through the welding point of the laminated body, and the main current is passed through the welding point of the laminated body for a period of time t 1 longer than the time period t that allows a large current to flow through the welding point of the laminated body 2 .

[0015] The method for manufacturing a welded structure according to the present disclosure is a method for manufacturing a welded structure formed by spot welding a laminated body formed of three or more metal plates stacked on each other, at least one of the three or more metal plates being thinner than the other metal plates, the method comprising: determining a method for welding the welded points to be welded based on the positions of the welded points to be welded, wherein, in the determination of the welding method, when the distance between the welded points to be welded and the welded points already welded exceeds a predetermined value, energizing the welded points of the laminated body while they are pressurized and causing a large current to flow through the welded points of the laminated body, and then spot welding the welded points of the laminated body while they are pressurized At the same time, power is continuously supplied so that a main current smaller than the large current flows through the welding points of the stack, and when the distance between the welding points to be welded and the welded welding points is a predetermined value or less, a welding method is used to weld the welding points to be welded, in which the welding points of the stack are energized while they are pressurized so that a matching current flows through the welding points of the stack, and then the welding points of the stack are continuously energized while they are pressurized so that a large current flows through the welding points of the stack, and then the welding points of the stack are continuously energized while they are pressurized and a main current smaller than the large current flows through the welding points of the stack, and the current value A13 of the matching current is smaller than the current value A11 of the main current.

[0016] The welding device according to the present disclosure is a welding device configured to spot weld a laminated body formed of three or more metal plates stacked on each other, at least one of the three or more metal plates being thinner than the other metal plates, the welding device comprising: an electrode configured to pressurize a welding point of the laminated body; a current generating circuit configured to cause a current to flow through the welding point of the laminated body pressed by the electrode; and a current control unit configured to perform a first control for maintaining the current as a main current and a second control for maintaining the current as a large current larger than the main current after maintaining the current as the main current by controlling the current generating circuit, wherein a time period t for causing the main current to flow through the welding point of the laminated body 1 longer than the time period t for causing the large current to flow through the welding point of the stacked body 2 .

[0017] A welding device according to the present disclosure is a welding device for spot welding a laminated body formed by three or more metal plates stacked on each other, at least one of the three or more metal plates being thinner than the other metal plates, the welding device comprising: an electrode configured to pressurize a welding point of the laminated body; a current generating circuit configured to cause current to flow through the welding point of the laminated body pressurized by the electrode; and a current control unit configured to perform a first control for maintaining the current at a matching current, a second control for maintaining the current at a large current after maintaining the current at the matching current, and a third control for maintaining the current at a main current smaller than the large current after maintaining the current at the large current by controlling the current generating circuit, wherein the matching current is smaller than the main current.

[0018] According to the present disclosure, the formation of burrs can be reduced.

[0019] The above and other objects, features and advantages of the present disclosure will become more fully understood from the detailed description given below and the accompanying drawings which are given by way of illustration only and therefore should not be regarded as limiting the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is a flow chart showing a method for manufacturing a welded structure according to a first embodiment;

[0021] Figure 2 is a schematic diagram showing one step of a method for manufacturing a welded structure according to a first embodiment;

[0022] Figure 3is a graph showing current variation in the method for manufacturing a welded structure according to the first embodiment;

[0023] Figure 4 is a schematic diagram showing the positional relationship between welded welding points and welding points to be welded;

[0024] Figure 5 is a flow chart showing a method for manufacturing a welded structure according to a second embodiment;

[0025] Figure 6 is a graph showing a change in current in a method for manufacturing a welded structure according to a second embodiment;

[0026] Figure 7 is a flow chart illustrating a method for manufacturing a welded structure according to a technique related to the present disclosure;

[0027] Figure 8 is a schematic diagram showing one step of a method for manufacturing a welded structure according to a technique related to the present disclosure;

[0028] Fig. 9 is a graph showing a current curve in a method for manufacturing a welded structure according to a technique related to the present disclosure; and

[0029] Fig.10 A photograph showing a burr formed in a welded solder joint. DETAILED DESCRIPTION

[0030] <Related Technology>

[0031] Before describing specific embodiments of the present invention, Figures 7 to 9 , a method for manufacturing a welded structure according to a technology related to the present disclosure will be described. Figure 7 is a flow chart illustrating a method for manufacturing a welded structure according to a technique related to the present disclosure.

[0032] Figure 8 yes Figure 7 A schematic diagram of a step in a method for producing a welded structure is shown. Fig. 9 It is shown Figure 7 A graph showing a current profile for use in a method for producing a welded structure is shown.

[0033] like Figure 7 and Figure 8As shown, the welding point P91 of the stacked body W910 is energized while it is pressurized, and a large current flows through the welding point P91 of the stacked body W910 (step ST91). Specifically, the stacked body W910 is formed by three or more metal plates stacked on each other, and at least one of the three or more metal plates is thinner than the other metal plates. Figure 8 An example of the stacked body W910 shown is formed by stacking metal plates W91, W92, and W93 one on another in this order. When electrodes E91 and E92 are kept pressed against welding point P91, a large current is caused to flow. A large current is caused to flow through welding point P91 of stacked body W910 for a period of time t 91 The current value of the large current is larger than the current value of the main current flowing in step ST92. Fig. 9 The current curve CA9 shown shows the change of the current value according to the manufacturing method. The current value of the large current is the current value A91.

[0034] Next, the welding point P91 of the laminated body W910 is continuously energized while being pressurized, and a main current is caused to flow through the welding point P91 of the laminated body W910 (step ST92). The current value of the main current is Fig. 9 The current value A92 is shown, and the current value A92 is smaller than the current value A91. Specifically, the current is reduced from the current value A91 to the current value A92, and the welding point P91 is continuously energized while it is pressurized. The main current is caused to flow through the welding point P91 of the stacked body W910 for a period of time t 92 In addition, the time period t 92 Longer than time period t 91 .

[0035] In the aforementioned method for manufacturing a welded structure according to the technology related to the present disclosure, burrs are often formed. Figure 8 As shown, in step ST91, a large current may flow through the welded welds WP91 and WP92 in a divided manner from the weld point P91 along the plane direction of the laminate W910 (in this example, the X-axis direction). When the current flows through the welded weld points WP91 and WP92 in a divided manner, burrs are generally formed in the weld point P91. In addition, when the distance between the weld point P91 and the welded weld points WP91 and WP92 is short, the current may flow through the welded weld points WP91 and WP92 in a divided manner, and burrs may be formed in the weld point P91.

[0036] The applicant has conceived the present disclosure through intensive research on various factors such as current magnitude, time period, sequence, etc., focusing on the fact that current has an influence on the formation of burrs.

[0037] Below, in conjunction with the accompanying drawings, a specific embodiment of the present disclosure is described in detail. However, the present disclosure is not limited to the following embodiments. In addition, for the sake of clarity of the description, the following description and the accompanying drawings are appropriately simplified.

[0038] <First Embodiment>

[0039] refer to Figures 1 to 4 , the first embodiment will be described. Figure 1 is a flowchart illustrating a method for manufacturing a welded structure according to a first embodiment. Figure 2 yes Figure 1 A schematic diagram of a step in a method for producing a welded structure is shown. Figure 3 It is shown Figure 1 A graph showing the variation of current in a method for producing a welded structure is shown. Figure 4 It is a schematic diagram of the positional relationship between welded welding points and welding points to be welded.

[0040] Of course, for convenience, use Figure 2 The right-handed XYZ coordinate system shown in the other figures is used to illustrate the positional relationship between the components. Generally, as commonly seen in the figures, the positive direction of the Z axis is the vertical upward direction, and the XY plane is a horizontal plane.

[0041] In the method for manufacturing a welded structure according to the first embodiment, it is possible to use Figure 2 The welding device E10 shown. The welding device E10 includes electrodes E1 and E2, a current generating circuit E3 and a control unit E4. The electrodes E1 and E2 are clamped by a moving arm or the like (not shown) so that they can move. The electrodes E1 and E2 pressurize the welding point P1 of the stack W10 by holding the welding point P1 of the stack W10 by the moving arm or the like and squeezing the welding point P1 of the stack W10. The current generating circuit E3 is electrically connected to a power source (not shown) and generates current from the power source. The current generating circuit E3 causes current to flow through the welding point P1 of the stack W10 pressurized by the electrodes E1 and E2. The control unit E4 can control the operation of the electrodes E1 and E2 via the moving arm or the like. The control unit E4 includes a current control unit E41. The current control unit E41 is capable of controlling the current generating circuit E3 and changing the magnitude of the current flowing in the current generating circuit E3 over time.

[0042] like Figure 2 As shown, the welding point P1 of the stack W10 is energized while it is pressurized, and the main current is caused to flow through the welding point P1 of the stack W10 (step ST1). Specifically, the stack W10 is formed by three or more metal plates stacked on each other. In addition, in the stack W10, at least one metal plate among the three or more metal plates is thinner than the other metal plates. That is, the stack W10 is a plate group with a high plate thickness ratio. Figure 2An example of a laminated body W10 shown in FIG. 1 is formed of metal plates W1, W2, and W3 stacked one on top of another in sequence. The metal plate W3 is thinner than the metal plates W1 and W2. The metal plates W1, W2, and W3 may be, for example, steel plates of different types from one another. When the electrodes E1 and E2 are kept pressed against the welding point P1, the main current is caused to flow. Figure 2 and Figure 3 As shown, the main current is in the time period t 1 The electrodes E1 and E2 are preferably electrically connected to a power source (not shown). The power source preferably allows current to flow through the stack W10 via the electrodes E1 and E2 as appropriate. In addition, the diameters of the electrodes E1 and E2 and the welding pressure at which the electrodes E1 and E2 press the welding point P1 can be appropriately selected based on widely used standards.

[0043] Furthermore, in time period t 1 During this period, the main current is passed through the welding point P1 of the laminate W10, and during the time period t 2 During this time, a large current is passed through the welding point P1 of the laminate W10. 1 Preferably longer than the time period t 2 , making it impossible for burrs to form.

[0044] like Figure 4 As shown, the distance L1 between the welding point P1 and the welded welding point WP1 and the distance L2 between the welding point P1 and the welded welding point WP2 can be appropriately determined. The distances L1 and L2 are not particularly limited and can be selected from a wide range of values ​​and can be, for example, 15 millimeters (mm) or 30 mm.

[0045] like Figure 2 As shown, when the main current is made to flow through the welding point P1 of the laminate W10 in step ST1, the main current flows through the welding point P1 and flows along the thickness direction of the laminate W10 (in this example, the Z direction). The current-carrying path is ensured so that the current passes through the welding point P1 and the laminate W10 from the electrode E1 and flows through the electrode E2. The nugget N1 is formed inside the laminate W10 from the welding point P1 of the laminate W10. Specifically, the nugget N1 is formed in the metal plate W1 and the metal plate W2. The nugget N1 mainly grows in the plane direction of the laminate W10 (in this example, the XY direction). In step ST1, in many cases, the nugget N1 grows inside the metal plate W1 and the metal plate W2, but the nugget N1 does not reach the inside of the metal plate W3.

[0046] Next, after step ST1, the welding point P1 of the laminate W10 is continuously energized while it is pressurized, and a large current is caused to flow through the welding point P1 of the laminate W10 (step ST2). Specifically, the current is increased from the current value A1 to the current value A2, and the welding point P1 is continuously energized while it is pressurized. Figure 2 and Figure 3 As shown, in the time period t 2 In the embodiment, a large current is caused to flow through the welding point P1 of the laminated body W10 at a current value A2. Therefore, the nugget N1 grows so that it reaches the inside of the metal plate W3. As a result, the nugget N1 grows inside the metal plates W1, W2, and W3 so that the nugget N1 has a sufficiently large size.

[0047] Figure 3 The current curve CA1 shown in FIG. 1 shows the change of the current value according to the manufacturing method. Figure 3 As shown, the current value A1 of the main current is smaller than the current value A2 of the large current. The current ratio A2 / A1 of the current value A2 to the current value A1 may be, for example, 1.4 or more, and more specifically, 1.4 or more and 1.7 or less. The current value A2 may be, for example, 11 kiloamperes (kA) or more, and more specifically, 12 kA or more. Even when the thickness of the metal plate W3 is small, welding can be performed with high welding quality.

[0048] In addition, the time period t 1 Preferably longer than the time period t 2 , making it impossible to form burrs. In addition, the time period t 1 Preferably, the time period t 2 1.00 times or more, and more preferably the time period t 2 2.50 times or more. In addition, the time period t 1 Preferably, the time period t 2 2.8 times or more, but not more than 5.0 times. In addition, the time period t 2 Preferably, it is 4 cycles (cyc) or more and 7 cyc or less. By defining the time period t in this way 1 The scope and time period t 2 range, the formation of burrs can be further reduced.

[0049] As can be seen from the above description, the nugget N1 solidifies, and the metal plates W1, W2, and W3 of the stacked body W10 are welded together. That is, a welded structure in which the metal plates W1, W2, and W3 of the stacked body W10 are welded together can be manufactured. In the aforementioned method for manufacturing a welded structure according to the first embodiment, the main current and the large current are less likely to flow from the welding point P1 through the welding points WP1 and WP2 separately in the plane direction of the stacked body W10, but flow from the welding point P1 in the thickness direction of the stacked body W10. Therefore, the formation of burrs at the welding point P1 can be reduced.

[0050] also, Figure 4 The distances L1 and L2 shown may be shorter. In this case, in the aforementioned method for manufacturing a welded structure according to the first embodiment, the main current and the large current are less likely to flow through the welded welds WP1 and WP2 separately from the weld point P1 in the plane direction of the laminate W10, but are likely to flow from the weld point P1 in the thickness direction of the laminate W10. As a result, the nugget N1 grows inside the metal plates W1, W2, and W3, and the metal plates W1, W2, and W3 are welded together with high welding quality. Therefore, burrs are less likely to be formed at the weld point P1. That is, at Figure 4 The above-described method for manufacturing a welded structure according to the first embodiment is preferred when the distances L1 and L2 shown in FIG. 1 are also short.

[0051] <Second Embodiment>

[0052] refer to Figure 2 , Figure 5 and Figure 6 , the second embodiment will be described. Figure 5 is a flowchart illustrating a method for manufacturing a welded structure according to a second embodiment. Figure 6 It is shown as Figure 5 A graph showing the variation of current in a method for producing a welded structure is shown.

[0053] In the method for manufacturing a welded structure according to the second embodiment, similarly to the method for manufacturing a welded structure according to the aforementioned first embodiment, Figure 2 The welding device E10 is shown.

[0054] like Figure 2 As shown, the welding point P1 of the laminate W10 is energized while it is pressurized, and a matching current is caused to flow through the welding point P1 of the laminate W10 (step ST11). Specifically, the matching current is caused to flow while the electrodes E1 and E2 keep pressing the welding point P1. Figure 2 and Figure 6 As shown, the matching current is in the time period t 13The current A13 flows through the welding point P1 of the laminate W10. In addition, the diameters of the electrodes E1 and E2 and the welding pressure at which the electrodes E1 and E2 press the welding point P1 can be appropriately selected based on widely used standards.

[0055] When the matching current is caused to flow through the welding point P1 of the laminate W10 in step ST11, the matching current flows from the welding point P1 in the thickness direction of the laminate W10 (in this example, the Z direction). Therefore, the temperature of the laminate W10 increases and the resistivity of the laminate W10 decreases. The current-carrying path is fixed so that the current flows from the electrode E1 through the welding point P1 and the laminate W10 and through the electrode E2. Note that the nugget N1 is less likely to be formed in the laminate W10.

[0056] Next, the welding point P1 of the laminate W10 is continuously energized while it is pressurized, and a large current is caused to flow through the welding point P1 of the laminate W10 (step ST12). Specifically, the current is increased from the current value A13 to the current value A12, and the welding point P1 is continuously energized while it is pressurized. Figure 2 and Figure 6 As shown, in the time period t 12 In the embodiment of the present invention, a large current is caused to flow through the welding point P1 of the laminate W10 at a current value A12. Therefore, a nugget N1 appears in the laminate W10 and grows in the thickness direction (in this example, the Z-axis direction) of the laminate W10. As a result, the nugget N1 grows within the metal plates W1, W2, and W3.

[0057] Finally, the welding point P1 of the laminate W10 is continuously energized while it is pressurized, and the main current is caused to flow through the welding point P1 of the laminate W10 (step ST13). Specifically, the current is reduced from the current value A12 to the current value A11, and the welding point P1 is continuously energized while it is pressurized. Figure 2 and Figure 6 As shown, in the time period t 11 In the embodiment, the main current flows through the welding point P1 of the laminate W10 at the current value A11. Therefore, the nugget N1 grows in the plane direction (XY direction in this example) of the laminate W10. As a result, the nugget N1 grows inside the metal plates W1, W2 and W3 until the nugget N1 has a sufficiently large size.

[0058] Figure 6 The current curve CA2 shown in FIG. 1 shows the change of the current value according to the manufacturing method. Figure 6As shown, the current value A13 of the matching current is smaller than the current value A11 of the main current. The current value A11 of the main current is smaller than the current value A12 of the large current. The current ratio A13 / A11 of the current value A13 to the current value A11 is preferably, for example, 0.95 or less, and specifically, 0.65 or more and 0.95 or less. By limiting the range of the current ratio A13 / A11 in this way, the formation of burrs can be reduced.

[0059] In addition, the time period t 11 It can be the time period t 12 2.50 times or more, and more preferably, the time period t 12 2.86 times or more but not more than 5.00 times. In addition, the time period t 11 It can be the time period t 13 3.00 times or less, and more preferably, the time period t 13 2.00 times or more but not more than 2.90 times. By defining the time period t in this way 11 , time period t 12 and time period t 13 , which can reduce the formation of burrs.

[0060] Through the above description, the nugget N1 is solidified, and the metal plates W1, W2, and W3 of the laminate W10 are welded together. That is, a welded structure in which the metal plates W1, W2, and W3 of the laminate W10 are welded together can be manufactured. In the aforementioned method for manufacturing a welded structure according to the second embodiment, the main current and the large current are less likely to flow through the welded welds WP1 and WP2 separately from the weld point P1 along the plane direction of the laminate W10, but flow from the weld point P1 along the thickness direction of the laminate W10. Therefore, the formation of burrs at the weld point P1 can be reduced.

[0061] [Example]

[0062] Next, an example of carrying out the method for manufacturing the welded structure according to each of the aforementioned first and second embodiments will be described.

[0063] In Examples 1-5, by using an example of the method for manufacturing a welded structure according to the first embodiment, a stacked body is welded together under the conditions shown in Table 1 below to manufacture a welded structure. Since a mild steel plate, a steel plate for hot stamping formed of a hot stamping material, and an ultra-high tensile strength steel plate are stacked on each other, a stacked body is formed. The detailed manufacturing conditions are as follows. That is, the thickness of the mild steel plate is 0.65 mm, the thickness of the steel plate for hot stamping is 1.8 mm, the thickness of the ultra-high tensile strength steel plate is 1.6 mm, the total plate thickness of the stacked body is 4.50 mm, the plate thickness ratio of the stacked body is 6.23, the diameter of the electrode is 6 mm, the welding pressure of the electrode squeezing the stacked body is 3820 kilonewtons (kN), and the distance between the welding point and the welded welding point is 15 mm. In Comparative Example 1, as shown in Table 1, except for the time period t during which a large current is allowed to flow, 2 Other than that, the manufacturing conditions were the same as those of Example 1.

[0064] In Examples 6-12, using an example of the method for manufacturing a welded structure according to the second embodiment, a stacked body is welded together under the conditions shown in Table 2 below to manufacture a welded structure. The stacked body has the same structure as in Examples 1-5. The specific manufacturing conditions are the same as in Examples 1-5. Note that in Comparative Examples 2-5, the manufacturing conditions are the same as in Examples 6-12 except for the current and time period shown in Table 2. For example, in Comparative Example 2, step ST11 is omitted.

[0065] The welding quality of the welding structure according to the examples and the comparative examples was evaluated. Specifically, when no burr was formed in the welding point of the welding structure in each of the examples and the comparative examples, the welding quality was evaluated as good (OK), and when the burr was formed, the welding quality was evaluated as bad (NG). Fig.10 A specific example B1 of the burr is shown. The evaluation results are shown in Tables 1 and 2.

[0066] [Table 1]

[0067]

[0068] In Examples 1-5, the evaluation was OK and no burr was formed. On the other hand, in Comparative Example 1, the evaluation was NG and burr was formed. One of the reasons for this is that the time period according to Comparative Example 1 is t 1 / t 2 It is 0.91, which is smaller than the value of Example 1-5.

[0069] [Table 2]

[0070]

[0071] In Example 6, the evaluation was OK and burrs were not formed. On the other hand, in Comparative Example 2, the evaluation was NG and burrs were formed. One of the reasons for this is that step ST11 was performed in Example 6, while step ST11 was not performed in Comparative Example 2.

[0072] In Examples 6-10, the evaluation was OK and no burr was formed. On the other hand, in Comparative Example 3, the evaluation was NG and burr was formed. One of the reasons for this is that the time period in Examples 6-10 was longer than t 11 / t 12 It is 2.86-5.00, which is larger than the value in Comparative Example 3.

[0073] In Example 11, the evaluation was OK and burrs were not formed. On the other hand, in Comparative Example 4, the evaluation was NG and burrs were formed. One of the reasons for this is that the current ratio A13 / A11 in Example 11 was 0.95, which was smaller than the value in Comparative Example 4.

[0074] In Example 12, the evaluation was OK and no burr was formed. On the other hand, in Comparative Example 5, the evaluation was NG and burr was formed. One of the reasons for this is that the time period in Example 12 was longer than t 11 / t 13 is 2.50, which is smaller than the value in Comparative Example 5.

[0075] Note that the present disclosure is not limited to the aforementioned embodiments, and can be appropriately changed without departing from the spirit of the present disclosure. In addition, the present disclosure can be performed by appropriately combining the aforementioned embodiments and one example thereof.

[0076] For example, the method for manufacturing a welded structure according to each of the aforementioned first and second embodiments may further include a step of determining a method for welding the welding point P1 to be welded based on the position of the welding point P1 to be welded.

[0077] In the step of determining the welding method, when the distances L1 and L2 between the welding point P1 to be welded and the already welded welding points WP1 and WP2 exceed predetermined values, the welding point P1 of the laminate W10 is energized while it is pressurized, and a large current is caused to flow through the welding point P1 of the laminate W10. The welding point P1 of the laminate W10 is continuously energized while it is pressurized, and a main current smaller than the large current is caused to flow through the welding point P1 of the laminate W10.

[0078] On the other hand, when the distances L1 and L2 are equal to or less than the predetermined value, steps ST1 and ST2 of the method for manufacturing a welded structure according to the first embodiment may be performed, and the welding point P1 to be welded may be welded.

[0079] Furthermore, when the distances L1 and L2 are equal to or less than the predetermined value, steps ST11 , ST12 , and ST13 in the method for manufacturing a welded structure according to the second embodiment may be performed, and the welding point P1 to be welded may be welded.

[0080] Furthermore, the control unit E4 of the welding device E10 may include a recording unit and a welding method determination unit. The recording unit records the distances L1 and L2 in advance. The welding method determination unit determines a method for welding the welding point P1 to be welded based on the distances L1 and L2.

[0081] From the above description, the method for manufacturing a welded structure according to each of the aforementioned first and second embodiments may further include a step of determining a method for welding the welded point P1 to be welded based on the position of the welded point P1 to be welded. In this case, the welded point P1 to be welded may be welded using a welding method according to the distances L1 and L2. Specifically, a welded point that is unlikely to form a burr may be welded using the method for manufacturing a welded structure according to the technology related to the present disclosure. On the other hand, a welded point that is likely to form a burr may be welded using the method for manufacturing a welded structure according to the first and second embodiments.

[0082] From the disclosure thus described, it will be apparent that the embodiments of the disclosure may be varied in many ways. Such variations should not be regarded as departing from the spirit and scope of the disclosure, and all such modifications obvious to those skilled in the art are intended to be included within the scope of the appended claims.

Claims

1. A method for manufacturing a welded structure, the welded structure being formed by spot welding a laminated body formed of three or more metal plates laminated on each other, at least one metal plate of the three or more metal plates being thinner than the other metal plates, the method comprising: applying a current to the welded point of the stacked body while applying pressure to the welded point, and causing a main current to flow through the welded point of the stacked body; as well as The welding point of the stacked body is continuously energized while the welding point is pressurized, and a large current greater than the main current flows through the welding point of the stacked body, Here, a time period (t1) during which the main current is passed through the welding point of the stacked body is longer than a time period (t2) during which the large current is passed through the welding point of the stacked body.

2. The method for manufacturing a welded structure according to claim 1, wherein: The time period (t1) during which the main current is passed through the welded point of the laminate is 2.50 times or more the time period (t2) during which the large current is passed through the welded point of the laminate.

3. The method for manufacturing a welded structure according to claim 1 or 2, wherein: The current value (A2) of the large current is 12 kA or more.

4. A method for manufacturing a welded structure, the welded structure being formed by spot welding a laminated body formed of three or more metal plates laminated on each other, at least one metal plate of the three or more metal plates being thinner than the other metal plates, the method comprising: applying a current to the welded point of the stack while applying pressure to the welded point, and passing a matching current through the welded point of the stack; The welding point of the stacked body is continuously energized while the welding point is pressurized, and a large current is passed through the welding point of the stacked body; as well as The welding point of the stacked body is continuously energized while the welding point is pressurized, and a main current smaller than the large current flows through the welding point of the stacked body, Wherein, the current value (A13) of the matching current is smaller than the current value (A11) of the main current.

5. The method for manufacturing a welded structure according to claim 4, wherein: The time period (t 11 ) is the time period (t 12 ) or more.

6. The method for manufacturing a welded structure according to claim 4 or 5, wherein: The time period (t 11 ) is the time period (t 13 ) is 3.00 times or less.

7. The method for manufacturing a welded structure according to claim 4 or 5, wherein: A current value (A13) of the matching current is 0.95 times or less of a current value (A11) of the main current.

8. The method for manufacturing a welded structure according to claim 1 or 4, wherein The stack includes welded weld points that have been welded, and The weld point of the stack is within 15 mm of the welded weld point.

9. A method for manufacturing a welded structure formed by spot welding a laminated body formed of three or more metal plates laminated on each other, at least one metal plate among the three or more metal plates being thinner than the other metal plates, the method comprising: Based on the position of the welding point to be welded, a method for welding the welding point to be welded is determined, wherein When determining a method for welding the welding point to be welded, When the distance between the welding point to be welded and the already welded welding point exceeds a predetermined value, the welding point of the stack is electrified while the welding point is pressurized and a large current flows through the welding point of the stack, and then the welding point of the stack is continuously electrified while the welding point is pressurized and a main current smaller than the large current flows through the welding point of the stack, and When the distance between the welding point to be welded and the welded welding point is a predetermined value or less, the welding point to be welded is welded by the following welding method, in which the welding point of the stack is energized while the welding point is pressurized and the main current flows through the welding point of the stack, and then the welding point of the stack is continuously energized while the welding point is pressurized and a large current greater than the main current flows through the welding point of the stack, and the time period (t1) during which the main current flows through the welding point of the stack is longer than the time period (t2) during which the large current flows through the welding point of the stack.

10. A method for manufacturing a welded structure formed by spot welding a laminated body formed of three or more metal plates laminated on each other, at least one metal plate among the three or more metal plates being thinner than the other metal plates, the method comprising: Based on the position of the welding point to be welded, a method for welding the welding point to be welded is determined, wherein When determining a method for welding the welding point to be welded, When the distance between the welding point to be welded and the already welded welding point exceeds a predetermined value, the welding point of the stack is energized while the welding point is pressurized and a large current flows through the welding point of the stack, and the welding point of the stack is continuously energized while the welding point is pressurized and a main current smaller than the large current flows through the welding point of the stack, and When the distance between the welding point to be welded and the welded welding point is a predetermined value or smaller, the welding point to be welded is welded by the following welding method, in which the welding point of the stack is energized while the welding point is pressurized, a matching current flows through the welding point of the stack, and then the welding point of the stack is continuously energized while the welding point is pressurized and a large current flows through the welding point of the stack, and then the welding point of the stack is continuously energized while the welding point is pressurized and a main current smaller than the large current flows through the welding point of the stack, and the current value (A13) of the matching current is smaller than the current value (A11) of the main current.

11. A welding device configured to spot weld a laminated body formed of three or more metal plates laminated on one another, at least one metal plate among the three or more metal plates being thinner than the other metal plates, the welding device comprising: an electrode configured to pressurize a weld point of the stack; a current generating circuit configured to cause current to flow through a welding point of the stacked body pressurized by the electrode; as well as a current control unit, the current control unit being configured to perform a first control and a second control by controlling the current generating circuit, wherein the first control is used to maintain the current as the main current, and the second control is used to maintain the current as a large current greater than the main current after maintaining the current as the main current, Here, a time period (t1) during which the main current is passed through the welding point of the stacked body is longer than a time period (t2) during which the large current is passed through the welding point of the stacked body.

12. A welding device for spot welding a laminated body formed by three or more metal plates laminated on each other, at least one metal plate among the three or more metal plates being thinner than the other metal plates, the welding device comprising: an electrode configured to pressurize a weld point of the stack; a current generating circuit configured to cause current to flow through a welding point of the stacked body pressurized by the electrode; as well as a current control unit, the current control unit being configured to perform first control, second control and third control by controlling the current generating circuit, wherein the first control is used to maintain the current at a matching current, the second control is used to maintain the current at a large current after maintaining the current at the matching current, and the third control is used to maintain the current at a main current smaller than the large current after maintaining the current at the large current, Wherein, the matching current is smaller than the main current.