Additive-equivalent composite manufacturing interface transition design method
By setting equal material bosses and stress relief holes in additive and other material composite manufacturing, and performing cleaning, preheating, stress relief and heat treatment, the problems of interface metallurgical defects and stress deformation are solved, and high-quality manufacturing of large and complex parts is achieved. performance and low-cost manufacturing.
Patent Information
- Application Number
- CN202410837839.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
AI Technical Summary
In composite manufacturing of materials such as additives, interface metallurgical defects and stress deformation control problems lead to low metallurgical quality and deformation problems of products, affecting the efficient, high-precision, low-cost manufacturing of high-performance large-scale complex parts.
By dividing the workpiece into equal material and additive parts, setting equal material bosses and processing at the interface, using finite element simulation calculations to design stress relief holes, controlling interface stress, and performing cleaning, preheating, stress relief and heat treatment to reduce metallurgical defects and stress.
It effectively suppresses interface metallurgical defects, reduces stress deformation, achieves metallurgical quality improvement and deformation control, and ensures high performance and low-cost manufacturing of parts.
Smart Images

Figure CN118720649A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of additive and isotropic composite manufacturing methods, and in particular to an additive and isotropic composite manufacturing interface transition design method. Background Art
[0002] Additive manufacturing technology is a process that uses three-dimensional model data as the basis to achieve part manufacturing by material accumulation. It is widely used in high-end equipment manufacturing fields such as aviation, aerospace, and military industry. As high-end equipment develops towards large-scale, lightweight, and integrated directions, low-cost and high-efficiency manufacturing of high-quality, high-reliability, and long-life large and complex parts poses new challenges to manufacturing technology.
[0003] At present, the manufacturing of large and complex parts has certain limitations. First, the overall additive manufacturing of large and complex parts faces the problems of high manufacturing costs and long delivery cycles. Second, the overall casting of large and complex parts faces the problems of uncontrollable local metallurgical defects and low product qualification rate. Third, large and complex parts are difficult to forge or spin as a whole.
[0004] To solve the above technical problems, a feasible method is to deeply integrate additive manufacturing technology (laser direct deposition, arc fuse additive manufacturing) with traditional equal material manufacturing technology (casting, forging, rolling, spinning), and use appropriate equal material manufacturing technology in parts with relatively simple structures, and use appropriate additive manufacturing technology in parts with relatively complex structures, so as to give full play to the respective technical advantages of additive manufacturing and equal material manufacturing and realize efficient and low-cost manufacturing of large and complex structures.
[0005] However, there are certain technical difficulties in additive manufacturing, mainly in the suppression of interface metallurgical defects and the control of interface stress and deformation. For example, when arc fuse additive manufacturing is used on the ZL205A high-strength aluminum alloy casting substrate to manufacture the local structure of high-strength aluminum alloy, defects such as dense pores are easily generated at the interface, which seriously affects the metallurgical quality of the product; for example, when laser direct deposition of titanium alloy local structure is used on the TC11 high-strength and tough titanium alloy forging substrate, stress concentration is easy to occur at the interface, resulting in large deformation or even cracking; arc fuse additive manufacturing of local structure on the 5B70 high-strength aluminum alloy spinning substrate is easy to occur stress concentration at the interface, resulting in deformation of the spinning part.
[0006] In view of this, how to effectively solve the problem of metallurgical defects and large stress deformation at the interface of additive manufacturing and isocratic material, so as to achieve efficient, high-precision and low-cost manufacturing of high-performance large-scale complex parts, has become an urgent problem to be solved in the development of additive manufacturing and engineering application. Summary of the invention
[0007] The purpose of the present invention is to provide a method for designing interface transition in additive manufacturing and isotropic composite manufacturing to solve the problems existing in the prior art.
[0008] To achieve the above object, the present invention provides the following solution: The present invention provides a method for designing interface transition for additive manufacturing and isotropic composite manufacturing, comprising the following steps:
[0009] S1: The workpiece is divided into a uniform material part and an additive material part, and an additive-uniform material interface is formed between the uniform material part and the additive material part; the workpiece is decomposed according to its own structural characteristics, the uniform material part corresponds to structural characteristics in the workpiece that are relatively simple and easy to obtain, such as a flat plate, a cylinder, a cone, etc., and the additive material part corresponds to structural characteristics in the workpiece that are relatively complex and difficult to obtain, such as a grid, a special-shaped structure, a thin wall, etc.
[0010] S2: Process the equal material part and process it into an equal material boss at the position of the equal material part close to the additive-equal material interface, and the equal material part is integrally arranged with the equal material boss; the equal material manufacturing process includes casting, forging, spinning, etc., which is determined according to the specific technical requirements and the structural form of the equal material part, such as casting, forging or rolling for flat plates, and spinning for rotating bodies such as cylinders and cones. Considering that the equal material part will undergo heat treatment together with the additive part later, in order to avoid coarse tissue, the equal material part is usually supplied in a hot-processed or cold-processed state. After the equal material part is processed, the shape quality inspection is carried out. The shape quality inspection includes geometric dimensions, shape and position tolerances, roughness, mechanical properties, surface quality inspection (visual inspection, penetration inspection), and internal quality inspection (ultrasonic inspection, X-ray inspection). Among them, the mechanical properties are the mechanical properties after heat treatment, and its heat treatment should be consistent with the final heat treatment system of the product. The geometric dimensions, shape and position tolerances and surface quality should meet the requirements of the process design drawings, and the mechanical properties and non-destructive testing should meet the product technical requirements.
[0011] S3: Processing the added material part on the equal material boss processed in step S2.
[0012] The beneficial effects of adopting the above technical solution are:
[0013] In order to suppress metallurgical defects, the present application sets an isomaterial boss on the isomaterial part corresponding to the additive-isomaterial interface, and the additive part is processed on the isomaterial boss, so that the processing area of the additive part is transformed from the entire upper surface of the isomaterial part to a local small surface area on the isomaterial boss, realizing the physical isolation of the isomaterial part and the additive part processing area, reducing the thermal influence of the energy beam heat input generated during the processing of the additive part on the microstructure and performance of the isomaterial part, thereby achieving the technical effect of suppressing metallurgical defects. In addition, the isomaterial boss can also provide a better heat dissipation boundary for the additive part processing area and provide better conditions for visually detecting metallurgical defects such as manufacturing boundary pores and unfused metallurgical defects.
[0014] Furthermore, in step S2: the height of the isotropic boss is 5 to 10 mm. A plurality of stress relief holes are formed on the isotropic boss. The stress relief holes can reduce the stress level of the reinforced-isotropic interface, thereby controlling deformation and inhibiting cracking. The size, depth and number of the stress relief holes are determined by finite element simulation calculation.
[0015] Furthermore, in step S3, before the additive part is processed, the equal-material part and the equal-material boss are cleaned and preheated; after the additive part is processed, the workpiece is subjected to stress relief and heat treatment.
[0016] The cleaning process includes: baking, grinding and wiping; baking the equal material part and the equal material boss, the baking temperature is 200-250°C, and the insulation time is 1-2 hours; after baking, grinding the equal material boss to remove the oxide scale on the surface of the equal material boss; after grinding, using anhydrous alcohol to remove dust on the surface of the equal material part and the equal material boss.
[0017] The preheating treatment includes: preheating the equal material part and the equal material boss by using a heating plate or a heating rope. When the equal material part and the equal material boss are made of aluminum alloy material, the preheating temperature is 80 to 120°C; when the equal material part and the equal material boss are made of titanium alloy material, the preheating temperature is 150 to 200°C.
[0018] The stress relief treatment is stress relief annealing or stress relief vibration. For large and complex parts, stress relief treatment needs to be performed within 24 hours after the additive processing is completed.
[0019] The heat treatment is carried out according to the heat treatment system after test verification and review of curing. A heating furnace that meets the requirements of GJB 509B or HB 5354 or other standards should be selected. For heat-treatable strengthening aluminum alloys, solid solution aging heat treatment is adopted, and the heating furnace category is not lower than Class II; for non-heat-treatable strengthening aluminum alloys, full annealing heat treatment is adopted, and the heating furnace category is not lower than Class III; for titanium alloys, double annealing is adopted, and the heating furnace category is not lower than Class III. According to the product design drawings and processing technical requirements, the machining procedures and processes are reasonably arranged, and the additive parts are rough-machined, semi-finished, and finished. Shape quality inspection includes geometric dimensions, form and position tolerances, roughness, mechanical properties, surface quality inspection (visual inspection, penetration inspection), and internal quality inspection (ultrasonic inspection, X-ray inspection). The geometric dimensions, form and position tolerances, and roughness should meet the requirements of the product design drawings; the mechanical properties are the mechanical properties of the parts after heat treatment, including the mechanical properties of the equal material part, the additive-equal material interface and the additive part. The sampling directions include the direction parallel to the deposition height increase direction (Z direction) and the direction perpendicular to the deposition height increase direction (X direction or Y direction). The test results should meet the product performance requirements; surface quality inspection and internal quality inspection shall be carried out in accordance with relevant standards and shall meet the product quality requirements.
[0020] Furthermore, the additive part is processed by laser direct deposition and / or arc fuse; according to the material and structure of the additive part, the appropriate additive part manufacturing process is selected; for titanium alloy or fine structure, laser direct deposition is used; for aluminum alloy or non-fine structure, arc fuse additive manufacturing is used. In order to avoid metallurgical defects and reduce the stress of the additive-isotope interface, the additive part manufacturing adopts a reciprocating continuous scanning track, the adjacent layer scanning tracks are orthogonal, and the track spacing is reasonable and suitable for overlap; the main process parameters of laser direct deposition include laser power, spot size, powder feeding speed, scanning speed, scanning spacing, etc. For titanium alloy, it is generally equipped with a deoxygenation and dehydration circulation purification system to ensure that the oxygen content of the manufacturing environment is ≤50ppm and the water content is ≤50ppm to avoid oxidation and hydrogen absorption; the main process parameters of arc fuse additive manufacturing include welding current, welding voltage, wire feeding speed, welding speed, interlayer temperature, track spacing, etc. For aluminum alloy, it is generally equipped with a heating and dehumidification circulation fan system to ensure that the relative humidity of the manufacturing environment is ≤50% to avoid the generation of pores. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is a structural diagram of a component according to Embodiment 1 of the present invention;
[0023] Figure 2 This is a schematic diagram of additive manufacturing according to Example 1 of the present invention;
[0024] Figure 3 This is a structural diagram of a component according to Embodiment 2 of the present invention;
[0025] Figure 4 This is a schematic diagram of additive manufacturing according to Embodiment 2 of the present invention;
[0026] Figure 5 This is a schematic diagram of additive manufacturing of a workpiece according to Embodiment 3 of the present invention;
[0027] Figure 6 It is a step diagram of the transition design method of the present invention;
[0028] Among them, 1. equal material part; 2. added material part; 3. equal material boss; 4. stress relief hole. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] Example 1
[0032] like Figure 1 As shown, this embodiment provides a ZL205A high-strength aluminum alloy cabin section reinforcement-equal material composite manufacturing interface transition design method.
[0033] The outline dimensions of the ZL205A high-strength aluminum alloy cabin are Φ819×437mm, the wall thickness is 19mm, and the net weight is 100kg. It is decomposed into two parts: the bottom cover plate and the upper cylinder. The bottom cover plate and the upper cylinder correspond to the equal material part 1 and the additive part 2 respectively. The bottom cover plate is made by casting, and the upper cylinder is made by additive processing.
[0034] The bottom cover plate is made of ZL205A cast plate. In order to meet the quality requirements of Class I castings, the cast plate is subjected to multiple hot rolling and supplied in a hot-processed state (without solution aging heat treatment).
[0035] The upper cylinder is manufactured by arc fuse additive manufacturing. The manufacturing platform is the arc fuse additive manufacturing system WAAM C1500 equipped with a heating and dehumidification circulating fan system. It is mainly composed of Fronius TPS 5000CMT welding power source, VR 1550CMT wire feeding device, RA 500022℃MT welding gun, RCU 5000i multi-function remote control box, ABB IRB 4600-40 / 2.55 robot, ICR5 robot control cabinet, dual-axis positioner, flexible workbench, dust removal system, environmental protection system, integrated control system, etc. The welding wire brand is ZL205A, the welding wire diameter is Φ1.2mm, and the main process parameters are: wire feeding speed 5.8~6.5m / min, welding speed 10mm / s, interlayer temperature ≤120℃, layer thickness 2mm, relative humidity ≤50%, dry extension 12~15mm; Zig-Zag reciprocating scanning is used to fill the track, the track spacing is 4mm, and the arc starting points or arc extinguishing points of adjacent layers are staggered.
[0036] like Figure 2 As shown, the height of the equal material boss 3 is 10mm. Combined with the finite element simulation calculation, the diameter of the stress release hole 4 is 5mm and the depth is 4mm. Before the additive manufacturing of the upper cylindrical arc fuse, the bottom cover plate and the equal material boss 3 are cleaned and preheated; the cleaning treatment first heats and bakes the bottom cover plate and the equal material boss 3 as a whole, and the corresponding parameters are 200℃ / insulation for 1h / air cooling. After the baking treatment, the equal material boss 3 is polished with an electric stainless steel wire brush to remove the surface oxide scale and expose the metal base color. Finally, anhydrous alcohol is used to wipe and remove the surface dust; the preheating treatment uses a heating rope to heat the bottom cover plate and the equal material boss 3, and the preheating temperature is 100℃.
[0037] After the additive manufacturing of the upper cylindrical arc fuse is completed, the part is first subjected to stress relief heat treatment, and the corresponding parameters are 320℃±10℃ / insulation for 30min / air cooling; then the part is subjected to rough machining and T6 solid solution aging heat treatment, and the corresponding parameters are: 538℃±5℃ / insulation for 12h / water quenching + 175℃±5℃ / insulation for 6h / air cooling, and the quenching transfer time does not exceed 20s; finally, the part is subjected to fine machining and shape quality inspection according to the design drawings, and the corresponding mechanical property test results meet the mechanical property requirements of QJ 3185-2003 "Specification for Aluminum Alloy ZL205A, ZL114A Castings for Aerospace Use", and the corresponding X-ray test results meet the requirements of Class I castings in QJ169A-2011 "Specification for Aluminum Alloy Castings", and there is no metallurgical quality problem and deformation at the additive-equal material interface.
[0038] Example 2
[0039] like Figure 3 As shown, this embodiment provides a TC11 high-strength and toughness titanium alloy suspension joint reinforcement-equal material composite manufacturing interface transition design method.
[0040] The TC11 high-strength and tough titanium alloy suspension joint has a size of 702×261×182mm, a wall thickness of 15mm, and a net weight of 27kg. It is decomposed into two parts: a bottom plate and an upper component. The bottom plate and the upper component correspond to the equal material part 1 and the additive part 2 respectively. The bottom plate is made by forging, and the upper component is made by additive manufacturing.
[0041] The bottom plate is made of TC11 forged plate, which is supplied in a hot-processed state (without annealing heat treatment). The upper components are manufactured by laser direct deposition additive manufacturing. The manufacturing platform is the laser additive manufacturing system LDM1500 with deoxygenation and dehydration circulation purification system, which is mainly composed of IPGYSL-4000 fiber laser, negative pressure powder feeder, YC52 laser cladding head, three-axis CNC machine tool, two-axis positioner, sealed box, purification and dust removal system, cooling system, integrated control system, etc. The powder material is TC11, with a particle size distribution of 75 to 250μm. The main process parameters are: laser power 2kw, spot diameter 2mm, powder feeding speed 20g / min, scanning speed 10mm / s, layer height 0.5mm, oxygen content ≤50ppm, water content ≤50ppm; Zig-Zag reciprocating scanning filling track, track spacing 1mm, adjacent layer tracks orthogonal.
[0042] like Figure 4 As shown in the figure, in the additive-isotropic material interface transition design, the height of the isotropic material boss 3 is 8mm. Combined with the finite element simulation calculation, the diameter of the stress release hole 4 is 4mm and the depth is 4mm. Before additive manufacturing, the bottom plate and isotropic material boss 3 are cleaned and preheated; the cleaning treatment first heats and bakes the bottom plate and isotropic material boss 3 as a whole, and the corresponding parameters are 200℃ / heat preservation for 1h / air cooling, and then the isotropic material boss 3 is polished with an electric stainless steel wire brush to remove the surface oxide scale and expose the metal base color, and finally the surface dust is wiped with anhydrous alcohol; the preheating treatment uses a heating rope to heat the bottom plate and isotropic material boss 3, and the preheating temperature is 180℃.
[0043] After the additive manufacturing of the upper component is completed, the parts are first subjected to stress relief heat treatment, with the corresponding parameters of 530℃±10℃ / insulation for 2h / air cooling; then the parts are subjected to rough machining and double annealing heat treatment, with the corresponding parameters of: 950℃±10℃ / insulation for 2h / air cooling + 550℃±10℃ / insulation for 6h / air cooling; finally, the parts are subjected to fine machining and shape quality inspection according to the design drawings, and the corresponding mechanical properties test results and X-ray test results meet the requirements of HB 20451-2018 "Specifications for Laser Direct Deposition Additive Manufacturing of Aviation Titanium Alloy Parts". There are no metallurgical quality problems and deformation at the additive-isotope interface.
[0044] Example 3
[0045] like Figure 5 As shown, this embodiment provides a method for designing interface transition of 5B70 high-strength aluminum alloy spun parts by adding equal materials to composite manufacturing.
[0046] The 5B70 high-strength aluminum alloy cabin has an outline size of Φ1080×460mm, a wall thickness of 15mm, and a net weight of 39kg. It is decomposed into a conical part and a local boss, corresponding to the equal-material part 1 and the added-material part 2, respectively.
[0047] The conical part is made of 5B70 spun parts and is supplied in a hot-processed state. The local boss is made of arc-fused additive manufacturing. The manufacturing platform is the arc-fused additive manufacturing system WAAM C1500 equipped with a heating and dehumidification circulation fan system. It mainly consists of Fronius TPS 5000CMT welding power source, VR 1550CMT wire feeder, RA500022℃MT welding gun, RCU 5000i multi-function remote control box, ABB IRB 4600-40 / 2.55 robot, ICR5 robot control cabinet, dual-axis positioner, flexible workbench, dust removal system, environmental protection system, integrated control system, etc. The welding wire brand is AlMgScZr, the welding wire diameter is Φ1.2mm, and the main process parameters are: wire feeding speed 3.8~4.5m / min, welding speed 6mm / s, interlayer temperature ≤100℃, layer thickness 1.5mm, relative humidity ≤50%, dry extension 12~15mm; Zig-Zag reciprocating scanning is used to fill the track, the track spacing is 4mm, and the arc starting points or arc extinguishing points of adjacent layers are staggered.
[0048] like Figure 5 As shown in the figure, in the additive-isotropic material interface transition design, the height of the isotropic material boss 3 is 5mm. Combined with the finite element simulation calculation, the diameter of the stress release hole 4 is 5mm and the depth is 5mm. Before additive manufacturing, the conical part and the isotropic material boss 3 are cleaned and preheated; the cleaning treatment first heats and bakes the conical part and the isotropic material boss 3 as a whole, and the corresponding parameters are 200℃ / heat preservation for 1h / air cooling, and then the isotropic material boss 3 is polished with an electric stainless steel wire brush to remove the surface oxide scale and expose the metal base color, and finally the surface dust is wiped with anhydrous alcohol; the preheating treatment uses a heating rope to heat the substrate, and the preheating temperature is 100℃.
[0049] After the local boss additive manufacturing is completed, the parts are fully annealed and heat treated, with the corresponding parameters of 320℃±10℃ / heat preservation for 30min / air cooling; then the parts are finely processed and the shape quality is tested according to the design drawings. The corresponding mechanical property test results and X-ray test results meet the product performance quality requirements, and the residual stress of the additive-equivalent material interface is less than 80MPa. There is no metallurgical quality problem and deformation at the additive-equivalent material interface.
[0050] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0051] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for designing interface transitions for additive manufacturing and isocratic composite manufacturing. It is characterized in that The following steps are involved: S1: dividing the workpiece into a uniform material portion (1) and an additive material portion (2), wherein an additive-uniform material interface is formed between the uniform material portion (1) and the additive material portion (2); S2: processing the equal material part (1) and processing the equal material part (1) at a position close to the increase-equal material interface to form an equal material boss (3), wherein the equal material part (1) and the equal material boss (3) are integrally arranged; S3: Processing the added material part (2) on the equal material boss (3) processed in step S2.
2. A method for designing interface transitions for additive manufacturing and isotropic composite manufacturing according to claim 1, It is characterized in that In the step S2: a plurality of stress release holes (4) are formed on the equal material boss (3).
3. A method for designing interface transitions for additive manufacturing and isotropic composite manufacturing according to claim 2, It is characterized in that The size, depth and number of the stress release holes (4) are determined by finite element simulation calculation.
4. The interface transition design method for additive manufacturing of isotropic composite materials according to claim 1, It is characterized in that In step S3, before the additive part (2) is processed, the equal material part (1) and the equal material boss (3) are cleaned and preheated; after the additive part (2) is processed, the workpiece is subjected to stress relief treatment and heat treatment.
5. The interface transition design method for additive manufacturing-isotope composite manufacturing according to claim 4, It is characterized in that The cleaning process comprises: baking, grinding and wiping; baking the equal material part (1) and the equal material boss (3), the baking temperature is 200-250° C., and the heat preservation time is 1-2 hours; after baking, grinding the equal material boss (3) to remove the oxide scale on the surface of the equal material boss (3); after grinding, using anhydrous alcohol to remove the dust on the surface of the equal material part (1) and the equal material boss (3).
6. The interface transition design method for additive manufacturing-isotope composite manufacturing according to claim 4, It is characterized in that The preheating treatment comprises: preheating the equal material part (1) and the equal material boss (3) by using a heating plate or a heating rope; when the equal material part (1) and the equal material boss (3) are made of aluminum alloy material, the preheating temperature is 80 to 120°C; when the equal material part (1) and the equal material boss (3) are made of titanium alloy material, the preheating temperature is 150 to 200°C.
7. The interface transition design method for additive manufacturing-isotope composite manufacturing according to claim 4, It is characterized in that The stress relief treatment is stress relief annealing or stress relief vibration.
8. The interface transition design method for additive manufacturing-isotope composite manufacturing according to claim 1, It is characterized in that The height of the equal material boss (3) is 5 to 10 mm.
9. The interface transition design method for additive manufacturing-isotope composite manufacturing according to claim 1, It is characterized in that The material addition part (2) is processed by direct laser deposition and / or arc fuse; the processing adopts a compound continuous scanning track, and the scanning tracks of adjacent layers are orthogonal.
Citation Information
Patent Citations
Additive manufacturing insert reinforced plate forming soft die structure and manufacturing method thereof
CN113145709A
Method for reducing residual stress of base material-additive body interface
CN113732305A
Equal material manufacturing-additive equal material composite manufacturing method and system for titanium alloy high-rib forgings
CN117182096A
Apparatus and methods for connecting nodes to panels in transport structures
US20190061835A1
Additive manufacturing process, additive layer, additive product, and composite laser
WO2022222590A1