Method for repairing flocked defective part

Through laser etching and glue repair technology, the problem of incomplete repair of flocking defective parts caused by manual trimming is solved, efficient repair of flocking defective parts is achieved, and economic losses and scrap rates are reduced.

CN118721803APending Publication Date: 2024-10-01ZHEJIANG HILDA AUTO PARTS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410746061.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When existing flocking technology is used to repair quality defects in automobile interior parts, manual trimming results in obvious repair marks, making it difficult to repair frontal defects, causing economic losses, and the repair scope is limited, making it impossible to effectively repair most products.

Method used

Laser etching technology is used to ablate the fluff and adhesive layer in the defective area, neatly exposing the base material, and limiting the adhesive patching area through baffles to ensure the quality of patch patching and achieve local patch patching operations.

Benefits of technology

Through laser etching and glue repair technology, the boundaries of repaired flocking defective parts are neat, which reduces the uncertainty of manual trimming, expands the repair scope, and significantly reduces the scrap rate of flocking parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721803A_ABST
    Figure CN118721803A_ABST
Patent Text Reader

Abstract

The invention discloses a method for repairing a flocked defective part, which comprises the following steps of: performing laser etching on a flocked defective area on the defective part, ablating fluff and an adhesive layer in the defective area according to a set shape, and ensuring that the boundary is tidy; performing glue filling on the etching area; and local complementary flocking operation is carried out. Local etching operation is carried out on the flocked defective part, the flock and the glue layer in the defective area are ablated through laser, the base material is exposed, the boundary of the adjacent areas on the periphery is neat and linear, the depth is consistent, follow-up flocked repair is greatly facilitated, and the rejection rate of the flocked part is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flocking, and in particular to a method for repairing a flocking defective part. Background Art

[0002] Flocking technology is becoming more and more mature, and flocking products are also widely used in many application fields. Flocking on clothing and accessories can create a luxurious visual effect. In recent years, it has been used more and more in automobiles. Flocking can reduce noise, increase friction, and change the visual effect.

[0003] Electrostatic flocking is one of the common flocking methods. It uses the principle of electrostatic field to make the villi and the plant body have opposite charges. It uses the principle that like charges repel each other and unlike charges attract each other to make the villi fly to the surface of the glue layer. The curing of the adhesive is used to stick the villi firmly to complete the flocking process.

[0004] Regardless of the flocking method, there are many factors that affect production, such as unskilled personnel, equipment failure, etc., and some products are always unqualified during production. Especially for automotive interior parts, the quality requirements are high. After quality defects occur, they can only be scrapped, resulting in a large quality loss. It is imperative to study the flocking repair technology of defective products.

[0005] For quality defects, currently the defect edges are trimmed with a manual knife, followed by glue filling and local flocking. However, since the trimming is done manually, the repair marks are obvious, and only the defects in the more hidden positions can be repaired. It is difficult to repair the front defects, and only a small part of the products can be saved, which still causes huge economic losses. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a method for repairing defective flocking parts, which can effectively repair most defective parts and reduce economic losses.

[0007] To this end, the technical solution of the present invention is: a method for repairing a flocking defective part, comprising the following steps:

[0008] 1) Laser etching is performed on the flocking defect area on the defective part, and the flock and glue layer in the defect area are ablated according to the set shape, and the boundary is neat;

[0009] 2) Fill the etched area with glue;

[0010] 3) Carry out local flocking work.

[0011] On the basis of the above scheme and as a preferred scheme of the above scheme: in step 1), the defective part is placed in a laser etcher to locate and determine the size of the defective area; then according to the size of the defective area, an etching range of appropriate size is selected and laser etching is performed to expose the substrate in the etched area.

[0012] On the basis of the above scheme and as a preferred scheme of the above scheme: the etching range is a circular area with different diameters, and the diameter of the circular area is 5 mm, 10 mm or 15 mm.

[0013] On the basis of the above scheme and as a preferred scheme of the above scheme: in step 2), a baffle is placed on the defective part, a glue filling hole is provided in the middle of the baffle, the glue filling hole is consistent in size with the etching area and is opposite in position; local glue filling is performed using a spray brush and the baffle.

[0014] On the basis of the above scheme and as a preferred scheme of the above scheme: in step 3), the local flocking operation uses the same specifications of the flock as other areas, and the flocking is flush with the surrounding area.

[0015] On the basis of the above scheme and as a preferred scheme of the above scheme: when there are multiple flocking defect areas on the defective part, the flocking defect areas are laser etched in turn; then the baffle is used to fill the glue on each etched area in turn; then all the glue-filled areas are flocked, and the flocking glue is cleaned and inspected after it is cured.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. For the flocking defective parts, local etching operation is adopted, and the hair and glue layer in the defective area are ablated by laser to expose the substrate, and the boundaries of the surrounding adjacent areas are neatly linear and the depth is consistent, which is very conducive to the subsequent flocking repair.

[0018] 2. Use the baffle to limit the flocking glue filling area to prevent other flocks from being stained with flocking glue and ensure the quality of the flocking filling.

[0019] 3. It effectively solves the glue spraying problem caused by inconsistent size of manual trimming, especially uneven edge lines, so that most of the flocking defective parts can be repaired, not limited to defects in hidden positions, greatly reducing the scrap rate of flocking parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A schematic diagram of a repair process for a single defect of the present invention;

[0021] Figure 2 This is a flowchart of the repair process of a single defect of the present invention;

[0022] Figure 3 It is a schematic diagram of the repair process of multiple defects of the present invention;

[0023] Figure 4 The figure is a flowchart of repairing multiple defects of the present invention.

[0024] Marked in the figure are: defective part 1, defective area 11, etching area 12, first etching area 13, second etching area 14, baffle 2, glue filling hole 21, first baffle 22, second baffle 23. DETAILED DESCRIPTION

[0025] In the description of the present invention, it should be noted that directional words, such as the terms "center", "lateral (X)", "longitudinal (Y)", "vertical (Z)", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", etc., indicating directions and positional relationships are based on the directions or positional relationships shown in the accompanying drawings, which are only for the convenience of narrating the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and cannot be understood as limiting the specific scope of protection of the present invention.

[0026] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features. Therefore, the definition of "first" and "second" features can explicitly or implicitly include one or more of the features. In the description of the present invention, "several" and "a number" mean two or more, unless otherwise clearly and specifically defined.

[0027] like Figure 1 , Figure 2 As shown, in the method for repairing a flocking defective part described in this embodiment, when there is only one defect on the defective part, the repair steps are as follows:

[0028] 1) Perform laser etching on the flocking defect area 11 on the defective part 1 to ablate the flock and glue layer in the defective area:

[0029] Using laser etching, put the defective flocked parts into the laser etcher, locate the shooting point, and then start the laser etcher. Set the etching range in the laser etcher, and the etching range can be selected into different circles with diameters of 5mm, 10mm, 15mm, etc. After the etcher etches, the fluff and glue layer of the defective area 11 can be burned away to expose the substrate, and the boundaries of the surrounding adjacent areas are neat and consistent. Since most flocking defects are caused by impurities, they rarely exceed 5mm; under normal circumstances, a 5mm circular etching area 12 will be left on the defective part 1.

[0030] 2) Fill the etched area 12 with glue:

[0031] A baffle 2 for shielding defective parts is prepared. The baffle 2 is cut from a 0.2-0.5 mm thick stainless steel plate. The shape of the baffle is irregular, but the area is larger than the etching area. At the same time, a glue filling hole 21 is provided on the baffle 2; different sizes of glue filling holes can be set on different baffles.

[0032] When filling the glue, select a suitable baffle 2 according to the size of the etched area 12 on the defective part 1, and place the baffle 2 above the defective part 1 so that the glue filling hole 21 is opposite to the etched area 12; then, use a spray pen to perform local glue filling, and the baffle 2 can prevent the flocking in other normal areas from being stained with glue; finally, remove the baffle 2, put it in water for cleaning, and put it dry for use.

[0033] 3) Carry out local flocking operation:

[0034] The defective part 1 after the repair is put into the flocking machine, and the flocking operation is performed with the same specifications of the flock, so that the flock falls into the etched area 12, is adhered by the flocking glue, and is flush with the surrounding area after flocking. Thus, the flocking repair work is completed. The flocking method here is consistent with the original flocking method of the defective part.

[0035] 4) After flocking, wait for the flocking glue to solidify, then clean and inspect.

[0036] like Figure 3 , 4 As shown in the figure, when there is only one defect on the defective part, the repair steps are as follows:

[0037] 1) Laser etching is performed on each flocking defect area 11 on the defective part 1 in turn to burn off the fluff and glue layer in the defective area 11; the defective flocking part is placed in a laser etcher, and the laser etcher performs shot point positioning and laser etching on each defective area to form each etching area.

[0038] 2) Fill the etched area with glue:

[0039] When filling glue, the etched areas on the defective part are covered and filled glue one by one. That is, firstly, the first baffle 22 is selected according to the size of the first etching area 13, and the first baffle 22 is placed above the defective part 1, so that the filling glue hole on the first baffle 22 is opposite to the first etching area 13; the first etching area 13 is filled glue by using a spray brush, and the first baffle 22 is removed after filling glue; then, the second baffle 23 is selected according to the size of the second etching area 14, and the second baffle 23 is placed above the defective part 1, so that the filling glue hole on the second baffle 23 is opposite to the second etching area 14; the second etching area 14 is filled glue by using a spray brush, and the second baffle 23 is removed after filling glue, and so on, to complete the filling glue operation of each etching area.

[0040] 3) Carry out local flocking operation:

[0041] Put the defective part after glue repair into the flocking machine, and use the same specification of flock to carry out flocking operation, so that the flock falls into each etched area, is adhered by the flocking glue, and is flush with the surrounding area after flocking. Thus, the flocking repair work is completed.

[0042] 4) After flocking, wait for the glue to solidify, then clean and inspect.

[0043] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for repairing a flocking defective part, characterized in that: The following steps are involved: 1) Laser etching is performed on the flocking defect area on the defective part, and the flock and glue layer in the defect area are ablated according to the set shape, and the boundary is neat; 2) Fill the etched area with glue; 3) Carry out local flocking work.

2. A method for repairing a flocking defective part according to claim 1, characterized in that: In step 1), the defective part is placed in a laser etcher to locate and determine the size of the defective area; then, according to the size of the defective area, an etching range of appropriate size is selected and laser etching is performed to expose the substrate in the etched area.

3. A method for repairing a flocking defective part according to claim 2, characterized in that: The etching range is a circular area with different diameters, and the diameter of the circular area is 5 mm, 10 mm or 15 mm.

4. A method for repairing a flocking defective part according to claim 1, characterized in that: In step 2), a baffle is placed on the defective part, a glue filling hole is provided in the middle of the baffle, and the glue filling hole is consistent in size with the etching area and is located opposite to the etching area; a spray brush and the baffle are used to perform local glue filling.

5. The method for repairing a flocking defective part according to claim 1, characterized in that: In step 3), the local flocking operation uses the same specifications of flock as other areas, and the flocking is flush with the surrounding area.

6. A method for repairing a flocking defective part according to claim 1, characterized in that: When there are multiple flocking defect areas on the defective part, the flocking defect areas are laser etched in turn; then the baffle is used to fill the glue on each etched area in turn; then all the glue-filled areas are flocked, and the flocking glue is cleaned and inspected after it is cured.

Citation Information

Patent Citations

  • An inner flock coating for vehicles with indicative and / or decorative motif and its manufacturing process

    CN101985263A