Preparation method of hollow composite carbon spheres

By in-situ coating of phenolic resin on the surface of hollow glass microspheres, the preparation process of hollow composite carbon spheres is simplified, the problems of agglomeration and uneven wall thickness are solved, and hollow composite carbon spheres with high sphericity and uniform wall thickness are achieved. , suitable for practical applications and industrial production.

CN118723969AActive Publication Date: 2024-10-01郑州坚峰复合材料有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410711712.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01
Estimated Expiration
2044-06-03

AI Technical Summary

Technical Problem

Existing preparation methods for hollow composite carbon spheres have problems such as agglomeration and uneven wall thickness, and require additional steps to remove templates and cumbersome fine control steps, which affects the realization of high sphericity.

Method used

Hollow glass microspheres are used as templates to prepare hollow composite carbon spheres by in-situ coating of phenolic resin-based materials, which simplifies the reaction process and avoids the template removal step. The mixed solution is added in batches to control the uniform coating of phenolic resin to ensure Sphericity and uniformity of wall thickness.

Benefits of technology

The preparation of hollow composite carbon balls with high sphericity and uniform wall thickness is achieved, simplifying the process, improving product stability and the feasibility of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723969A_ABST
    Figure CN118723969A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of carbon materials with special structures, and discloses a preparation method of hollow composite carbon spheres. The preparation method comprises the following steps: taking hollow glass beads as a hollow template, taking phenols and aldehydes as raw materials, under the action of a catalyst and a dispersing agent, synthesizing phenolic resin microspheres in situ at normal temperature, coating the phenolic resin microspheres on the surfaces of the hollow glass beads to form hollow composite phenolic resin spheres, and carbonizing to form the hollow composite carbon spheres. In the preparation process, pretreatment of the microspheres is not needed, additional steps for template removal are not needed, the prepared hollow composite carbon spheres are high in sphericity degree, and practical application and industrial production are better facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of special structure carbon materials, and in particular relates to a method for preparing hollow composite carbon spheres. Background Art

[0002] Hollow carbon spheres are a type of lightweight filler with a cavity structure and low density. They are widely used in catalysts, adsorbents, buoyancy materials and other fields.

[0003] The existing method for preparing porous hollow carbon spheres has some shortcomings. For example, the preparation of the silica template and the organic coating process are carried out step by step. In order to purify the template, it is necessary to undergo additional washing and separation processes. Before the coating process, the template needs to be ultrasonically treated to make it evenly dispersed. During the coating process, surfactants and reactants need to be added in multiple steps, the steps are cumbersome, and extremely fine regulation is required. After the coating is completed, since the silica template is a solid sphere, it is necessary to acid wash to remove the template.

[0004] At present, the hollow composite carbon spheres prepared by the existing technology have problems such as agglomeration and uneven wall thickness. Therefore, it is of great significance to develop a method for preparing hollow composite carbon spheres with high sphericity. Summary of the invention

[0005] The present invention proposes a method for preparing hollow composite carbon spheres by in-situ coating of phenolic resin-based carbon materials on the surface of hollow glass microspheres. The preparation process of this patent does not require the pre-treatment of microspheres, does not require the removal of templates, and the prepared hollow composite carbon spheres have high sphericity, which is more conducive to practical application and industrial production.

[0006] The purpose of the present invention is to provide a hollow composite carbon sphere with simple reaction process, environmental protection and high sphericity and a preparation method thereof.

[0007] The technical solution adopted by the present invention is a method for preparing hollow composite carbon spheres, which is specifically implemented according to the following steps:

[0008] A phenol source, a catalyst, hollow glass microspheres and water are mixed to prepare a mixed solution A; formaldehyde and a dispersant are mixed to prepare a mixed solution B;

[0009] Divide the mixed solution B into at least two portions, add one portion of the mixed solution B to the mixed solution A each time, and mix and stir until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C;

[0010] Drying the mixed solution C to obtain hollow composite phenolic resin balls, wherein the hollow composite phenolic resin balls include hollow glass microspheres and phenolic resin coated on the hollow glass microspheres;

[0011] The hollow composite phenolic resin balls are sintered to obtain hollow composite carbon balls, which include hollow glass microspheres and a carbon layer covering the hollow glass microspheres.

[0012] In this way, hollow composite carbon spheres are prepared by using hollow glass microspheres as templates and in-situ coating of phenolic resin microspheres on the surface of the templates. No additional steps are required to remove the templates, and a dispersant is introduced to make the synthesized hollow composite carbon spheres have good stability, high monodispersity, and no adhesion to each other. At the same time, by controlling the synthesis method of the mixed solution C, a portion of the mixed solution B is added to the mixed solution A first, and then the remaining mixed solution B is added. After each addition, the synthesized phenolic resin microspheres are in-situ grown on the surface of the hollow glass microspheres. Slow mixing can make the prepared phenolic resin microspheres uniformly and densely coated on the surface of the hollow glass microspheres, avoiding the phenomenon of phenolic resin microspheres agglomerating with each other.

[0013] The present invention is also characterized in that:

[0014] In some embodiments, the mixed solution B is divided into at least two parts, and one part of the mixed solution B is added to the mixed solution A each time and mixed and stirred until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C. The mixing and stirring temperature is 15°C to 35°C and the stirring time is 0.5h to 1h each time the mixing is performed.

[0015] Preferably, the mixed solution B is composed of 2 parts of B1 and B2, and the ratio of B1:B2 is (1 / 5 to 1 / 2):(4 / 5 to 1 / 2) by mass. B1 is first added to the mixed solution A and mixed and stirred, and then B2 is divided into 1 to 10 parts, each added to the mixed solution A and mixed and stirred until the mixed solution B is completely mixed with the mixed solution A to obtain a mixed solution C.

[0016] Preferably, the mixed solution B2 is divided into 2 to 6 equal parts.

[0017] Thus, when mixed solution B is added to mixed solution A for the first time, the phenolic resin microspheres generated by phenol source and formaldehyde are coated on the surface of hollow glass microspheres by slow stirring, and the microspheres are closely arranged to form a dense phenolic resin microsphere layer. After the remaining mixed solution B is added to mixed solution A for mixing each time, a layer of phenolic resin microspheres is uniformly coated on the surface of hollow composite phenolic resin balls to form a multilayer structure. A small amount of multiple additions and slow mixing and stirring process allow the newly generated phenolic resin microspheres to grow on the surface of hollow composite phenolic resin balls without forming agglomeration, thereby obtaining hollow composite phenolic resin balls with high sphericity and uniform wall thickness. In addition, the wall thickness obtained can be further controlled by controlling the amount of synthesized phenolic resin to obtain a hollow composite resin ball with controllable size.

[0018] In some embodiments, the mass ratio of phenol source, catalyst, hollow glass microspheres, water, formaldehyde and dispersant is (8-30):(6-20):(10-30):(100-200):(3-18):1.

[0019] Thus, the thickness of the carbon layer on the surface of the hollow glass microspheres can be adjusted by adjusting the amount of the synthesized phenolic resin, thereby adjusting the size of the hollow composite carbon spheres.

[0020] In some embodiments, the phenol source is selected from one or more of p-aminophenol, m-aminophenol, o-aminophenol, resorcinol, catechol, hydroquinone, and phloroglucinol.

[0021] In some embodiments, the dispersant is selected from one or more of Tween 80, Tween 60, polyvinyl alcohol, polypyrrolidone, polyethylene glycol, sodium dodecyl sulfonate, sodium dodecyl sulfate, hexadecyl ammonium bromide, OP-30, and triblock copolymer F127.

[0022] In some embodiments, the catalyst is selected from one or more of ammonia, triethylamine, sodium hydroxide, potassium hydroxide, barium hydroxide, magnesium hydroxide, and sodium carbonate.

[0023] In some embodiments, the size of the hollow glass microspheres is 1 to 100 um.

[0024] In some embodiments, the hollow composite phenolic resin balls are sintered, and the sintering process is firstly heating to 180-250° C. and maintaining for 0.5 h to 1 h, and then heating to 400-800° C. and maintaining for 1 h to 2 h.

[0025] Beneficial effects:

[0026] The present invention carries out the reaction in an efficient manner, that is, even if the mixed solution B is added to the mixed solution A in batches, the phenolic resin microspheres are prevented from sticking to each other during the synthesis process, and at the same time, the generated phenolic resin microspheres are uniformly coated on the surface of the hollow glass microspheres, thereby obtaining hollow composite phenolic resin balls with high sphericity, and obtaining hollow composite carbon balls with high sphericity after sintering and carbonization; the thickness of the carbon layer on the surface of the hollow glass microspheres can be adjusted by adjusting the amount of the synthesized phenolic resin, thereby adjusting the size of the hollow composite carbon balls, which is more conducive to practical application and industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The hollow glass microspheres are coated with phenolic resin microspheres obtained by the preparation method of the invention.

[0028] Figure 2 The present invention is a SEM image of a hollow composite carbon sphere with high sphericity obtained by the preparation method of the present invention. DETAILED DESCRIPTION

[0029] Example 1

[0030] S1: Respectively weigh resorcinol, ammonia water, hollow glass microspheres (D50=5 μm), water, formaldehyde and hexadecyl ammonium bromide in a mass ratio of 19:13:20:150:11:1; mix the weighed resorcinol, ammonia water, hollow glass microspheres and water to prepare a mixed solution A; mix formaldehyde and hexadecyl ammonium bromide to prepare a mixed solution B;

[0031] S2: First, 1 / 3 of the mixed solution B was mixed with the mixed solution A at 25°C and stirred for 0.8h, and then the remaining 2 / 3 of the mixed solution B was added in 3 batches, and each time the mixture was mixed and stirred at 25°C for 0.8h to obtain a mixed solution C. The mixed solution C was centrifuged, washed with water, and dried to obtain hollow composite phenolic resin balls; the hollow composite phenolic resin balls were first heated to 200°C in a tubular furnace and maintained for 0.8h, and then heated to 600°C and maintained for 1.5h to obtain hollow composite carbon balls.

[0032] Example 2

[0033] S1: p-aminophenol, triethylamine, hollow glass microspheres (D50=5 μm), water, formaldehyde and triblock copolymer F127 were weighed respectively in a mass ratio of 30:20:30:1200:18:1; the weighed p-aminophenol, triethylamine, hollow glass microspheres and water were mixed to prepare a mixed solution A; formaldehyde and triblock copolymer F127 were mixed to prepare a mixed solution B;

[0034] S2: First, 1 / 3 of the mixed solution B is mixed with the mixed solution A at 35°C for 1 hour, and then the remaining 2 / 3 of the mixed solution B is added in 3 batches, and each time the mixture is mixed and stirred at 35°C for 1 hour to obtain a mixed solution C. The mixed solution C is centrifuged, washed with water, and dried to obtain hollow composite phenolic resin balls; the hollow composite phenolic resin balls are first heated to 250°C in a tubular furnace and maintained for 1 hour, and then heated to 800°C and maintained for 2 hours to obtain hollow composite carbon balls.

[0035] Example 3

[0036] S1: weigh phloroglucinol, sodium hydroxide, hollow glass microspheres, water, formaldehyde and Tween 80 in a mass ratio of 8:6:10:100:3:1 respectively; mix the weighed phloroglucinol, sodium hydroxide, hollow glass microspheres and water to prepare a mixed solution A; mix formaldehyde and Tween 80 to prepare a mixed solution B;

[0037] S2: First, 1 / 3 of the mixed solution B was mixed with the mixed solution A at 15°C and stirred for 0.5h, and then the remaining 2 / 3 of the mixed solution B was added in 3 batches, and each time the mixture was mixed and stirred for 0.5h at 15°C to obtain a mixed solution C. The mixed solution C was centrifuged, washed with water, and dried to obtain hollow composite phenolic resin balls; the hollow composite phenolic resin balls were first heated to 180°C in a tubular furnace and maintained for 0.5h, and then heated to 400°C and maintained for 1h to obtain hollow composite carbon balls.

[0038] Example 4

[0039] S1: Respectively weigh resorcinol, ammonia water, hollow glass microspheres (D50=5 μm), water, formaldehyde and hexadecyl ammonium bromide in a mass ratio of 19:13:20:150:11:1; mix the weighed resorcinol, ammonia water, hollow glass microspheres and water to prepare a mixed solution A; mix formaldehyde and hexadecyl ammonium bromide to prepare a mixed solution B;

[0040] S2: First, 1 / 5 of the mixed solution B was mixed with the mixed solution A at 25°C and stirred for 0.8h, and then the remaining 4 / 5 of the mixed solution B was added in 5 batches, and each time the mixture was mixed and stirred at 25°C for 0.8h to obtain a mixed solution C. The mixed solution C was centrifuged, washed with water, and dried to obtain hollow composite phenolic resin balls; the hollow composite phenolic resin balls were first heated to 200°C in a tubular furnace and maintained for 0.8h, and then heated to 600°C and maintained for 1.5h to obtain hollow composite carbon balls.

[0041] Example 5

[0042] S1: Respectively weigh resorcinol, ammonia water, hollow glass microspheres (D50=5 μm), water, formaldehyde and hexadecyl ammonium bromide in a mass ratio of 19:13:20:150:11:1; mix the weighed resorcinol, ammonia water, hollow glass microspheres and water to prepare a mixed solution A; mix formaldehyde and hexadecyl ammonium bromide to prepare a mixed solution B;

[0043] S2: First, 1 / 2 of the mixed solution B was mixed with the mixed solution A at 25°C and stirred for 0.8h, and then the remaining 1 / 2 of the mixed solution B was added in 2 batches, and each time the mixture was mixed and stirred at 25°C for 0.8h to obtain a mixed solution C. The mixed solution C was centrifuged, washed with water, and dried to obtain hollow composite phenolic resin balls; the hollow composite phenolic resin balls were first heated to 200°C in a tubular furnace and maintained for 0.8h, and then heated to 600°C and maintained for 1.5h to obtain hollow composite carbon balls.

[0044] Example 6

[0045] S1: Respectively weigh resorcinol, ammonia water, hollow glass microspheres (D50=5 μm), water, formaldehyde and hexadecyl ammonium bromide in a mass ratio of 19:13:20:150:11:1; mix the weighed resorcinol, ammonia water, hollow glass microspheres and water to prepare a mixed solution A; mix formaldehyde and hexadecyl ammonium bromide to prepare a mixed solution B;

[0046] S2: First, 1 / 2 of the mixed solution B is mixed with the mixed solution A at 25°C and stirred for 0.8h, and then the remaining 1 / 2 of the mixed solution is added, and mixed and stirred at 25°C for 0.8h to obtain a mixed solution C. The mixed solution C is centrifuged, washed with water, and dried to obtain hollow composite phenolic resin balls; the hollow composite phenolic resin balls are first heated to 200°C in a tubular furnace and maintained for 0.8h, and then heated to 600°C and maintained for 1.5h to obtain hollow composite carbon balls.

[0047] Comparative Example 1

[0048] The difference from Example 1 is that:

[0049] The preparation method of mixed solution C is as follows: firstly, 2 / 3 of mixed solution B and mixed solution A are mixed and stirred at 25° C. for 0.8 h; and then the remaining 1 / 3 of mixed solution B is added in 3 batches. The rest is the same as in Example 1.

[0050] Comparative Example 2

[0051] The difference from Example 1 is that:

[0052] The mixing method of the mixed solution C is as follows: taking all the mixed solution B and the mixed solution A, mixing and stirring at 25° C. for 0.8 h to obtain the mixed solution C. The rest is the same as in Example 1.

[0053] Test method: The wall thickness of the hollow composite carbon spheres in the TEM image was measured, and the standard deviation of the wall thickness was obtained by calculation.

[0054] (1) Take one hollow composite carbon sphere from each group of samples, and take 10 points on each hollow composite carbon sphere to measure the wall thickness. Calculate the standard deviation of wall thickness for each group;

[0055] (2) Take 50 hollow composite carbon balls from each group of samples, and take one point on each of the 50 hollow composite carbon balls to measure the wall thickness. Calculate the standard deviation of wall thickness for each group;

[0056] (3) Calculate the equivalent diameter of the largest particle when the cumulative distribution is 50% in each set of particle size distribution curves.

[0057] Test results:

[0058]

[0059] Embodiment 1-3 adjusts the proportion of each component, uses hollow glass microspheres with the same particle size, and the prepared hollow composite carbon spheres have high sphericity, and the diameter increases with the increase of the amount of raw material added. Embodiment 4-5 adjusts the mixing mode of mixed solution A and mixed solution B, and changes the amount of phenolic resin generated by each mixing compared with embodiment 1. The wall thickness standard deviation and equivalent diameter of the prepared hollow composite carbon spheres are slightly increased for embodiment 1. Embodiment 6 reduces the number of times mixed solution B is added to mixed solution A. Due to the mixing and stirring after each addition, the amount of phenolic resin microspheres generated is relatively large, which makes some phenolic resin balls agglomerate with each other to a certain extent, reducing the uniformity of the phenolic resin microsphere layer of the outer layer of the hollow glass microspheres. Therefore, the wall thickness standard deviation and equivalent diameter of the prepared hollow composite carbon spheres are slightly increased for embodiment 1.

[0060] Compared with Example 1, Comparative Examples 1-2 use the same amount of resin coating. Comparative Examples 1-2 change the addition method of mixed solution A and mixed solution B, resulting in poor coating effect of phenolic resin microspheres on hollow glass microspheres, uneven wall thickness of the prepared hollow composite carbon spheres, and unstable size.

[0061] Although the present invention has been described in detail by reference to the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. A method for preparing hollow composite carbon spheres, characterized in that: Follow the steps below to implement it: A phenol source, a catalyst, hollow glass microspheres and water are mixed to prepare a mixed solution A, and formaldehyde and a dispersant are mixed to prepare a mixed solution B; Divide the mixed solution B into at least two portions, add one portion of the mixed solution B to the mixed solution A each time, and mix and stir until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C; Drying the mixed solution C to obtain hollow composite phenolic resin balls, wherein the composite phenolic resin balls include hollow glass microspheres and phenolic resin coated on the hollow glass microspheres; The hollow composite phenolic resin spheres are sintered to obtain hollow composite carbon spheres.

2. The method for preparing hollow composite carbon spheres according to claim 1, characterized in that: The step of dividing the mixed solution B into at least two portions, adding one portion of the mixed solution B to the mixed solution A each time and mixing and stirring until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C also includes that each time the mixing is performed, the mixing and stirring temperature is 15° C. to 35° C., and the stirring time is 0.5 h to 1 h.

3. The method for preparing hollow composite carbon spheres according to claim 2, characterized in that: The mixed solution B is first divided into two parts, B1 and B2, and the ratio of B1:B2 is (1 / 5-1 / 2):(4 / 5-1 / 2) by mass fraction. B1 is first added to the mixed solution A and mixed and stirred, and then B2 is divided into 1-10 parts, added to the mixed solution A and mixed and stirred until the mixed solution B and the mixed solution A are completely mixed to obtain a mixed solution C.

4. The method for preparing hollow composite carbon spheres according to claim 3, characterized in that: The mixed solution B2 was divided into 2 to 6 equal parts, and then the mixed solution A was added and mixed and stirred.

5. The method for preparing hollow composite carbon spheres according to claim 1, characterized in that: The mass ratio of the phenol source, catalyst, hollow glass microspheres, water, formaldehyde and dispersant is (8-30):(6-20):(10-30):(100-200):(3-18):

1.

6. The method for preparing hollow composite carbon spheres according to claim 1, characterized in that: The phenol source is selected from one or more of p-aminophenol, m-aminophenol, o-aminophenol, resorcinol, catechol, hydroquinone and phloroglucinol.

7. The method for preparing hollow composite carbon spheres according to claim 1, characterized in that: The dispersant is selected from one or more of Tween 80, Tween 60, polyvinyl alcohol, polypyrrolidone, polyethylene glycol, sodium dodecyl sulfonate, sodium dodecyl sulfate, hexadecyl ammonium bromide, OP-30, and triblock copolymer F127; the catalyst of the hollow composite carbon sphere is selected from one or more of ammonia water, triethylamine, sodium hydroxide, potassium hydroxide, barium hydroxide, and magnesium hydroxide.

8. The method for preparing hollow composite carbon spheres according to claim 1, characterized in that: The particle size of the hollow glass microbeads is 1 to 100 um.

9. The method for preparing hollow composite carbon spheres according to claim 1, characterized in that: The hollow composite phenolic resin balls are sintered, and the sintering process is firstly heating to 180-250° C. and keeping for 0.5 h-1 h, and then heating to 400-800° C. and keeping for 1 h-2 h.

10. A hollow composite carbon sphere, characterized in that: Prepared by the method according to any one of claims 1 to 9, the hollow composite carbon spheres include hollow glass microspheres and a carbon layer coated on the hollow glass microspheres; The outer diameter of the carbon layer is 3-106 μm, the inner diameter is 1-100 μm, and the thickness of the carbon layer is 1-3 μm.

Citation Information

Patent Citations

  • Composite hollow microsphere and preparation method and application thereof

    CN103665747A

  • Simple and convenient resorcinol formaldehyde resin hollow composite material and preparing method of derivative thereof

    CN105061705A

  • Microwave preparation method for monodisperse size-adjustable hollow porous carbon-spheres

    CN106167255A

  • Hollow glass bead cladded with phenolic resin, and preparation method of hollow glass bead

    CN108822581A

  • Single-layer and multi-layer hollow carbon nanosphere, and preparation and application thereof

    WO2016150406A1