Process for preparing sodium bromide from DMAC cuprous bromide hazardous waste and application

High-purity sodium bromide is prepared through the process of DMAC cuprous bromide hazardous waste, which solves the problems of hazardous cuprous bromide waste treatment and bromine element recovery, and achieves efficient resource utilization and environmental protection.

CN118724019APending Publication Date: 2024-10-01ZHEJIANG HONGDIAN ENVIRONMENTAL PROTECTION EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410946160.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technologies fail to effectively process and recycle hazardous wastes of cuprous bromide, resulting in environmental pollution and resource waste, and do not realize the recycling of bromine elements.

Method used

The process of preparing sodium bromide using DMAC cuprous bromide hazardous waste includes preliminary sorting, grinding and pretreatment, reduction reaction, separation and purification, electrolytic preparation and dehydration and drying. Through the reduction reaction of zinc powder reducing agent and urea, high Preparation of pure sodium bromide.

Benefits of technology

It realizes the preparation of high-purity sodium bromide with high recycling rate, solves the problem of environmental pollution, creates economic value, and is suitable for organic solvent systems of halogen compounds containing catalytic metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724019A_ABST
    Figure CN118724019A_ABST
Patent Text Reader

Abstract

The invention discloses a process for preparing sodium bromide from DMAC cuprous bromide hazardous waste and application. According to the process, the high-purity sodium bromide crystal is prepared from cuprous bromide hazardous waste, can be used for preparing other bromine-containing compounds, and has a wide application prospect. The bromine is prepared in an electrolysis mode, equipment is simple, operation is easy, the electrolysis efficiency is high, the bromine recycling rate is larger than 99%, sodium hypobromite in the solution is reduced through urea, the high-purity sodium bromide mother liquor is prepared, the high-purity sodium bromide crystals are further prepared through dehydration and drying, the process operation is simple, the reaction efficiency is high, and the prepared product is high in purity and high in recycling rate. The method provided by the invention not only improves the utilization rate of the raw materials, but also realizes efficient recovery of each substance, has good application prospect and popularization value, and is suitable for treating an organic solvent system containing catalytic metal halide compounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hazardous waste treatment, and specifically relates to a production process for preparing sodium bromide by utilizing DMAC (dimethylacetamide) cuprous bromide hazardous waste, and application of the production process. Background Art

[0002] In the context of industrial development, the generation and treatment of cuprous bromide hazardous waste has become an urgent issue. Cuprous bromide hazardous waste mainly comes from waste catalysts in organic synthesis reactions, which are widely used in alkylation reactions of brominated acyl chlorides, coupling nitrogen reactions, and photosensitizer components in the photographic industry. In addition, cuprous bromide is also used in catalytic reactions in other organic chemistry research.

[0003] Traditional methods for treating cuprous bromide hazardous waste include landfill and incineration, but these methods are inefficient and may cause secondary pollution to the environment. Specifically:

[0004] 1. Landfill method: It involves the safe landfill of cuprous bromide hazardous waste. It is necessary to select a suitable site and follow relevant standards for design and construction to reduce the impact on the environment.

[0005] 2. Incineration method: Through high-temperature decomposition and deep oxidation processes, cuprous bromide hazardous waste is converted into harmless substances, reducing the waste volume and removing toxicity, but attention should be paid to the treatment of waste gas and waste residue generated by incineration.

[0006] 3. Chemical method: Use chemical reactions to convert cuprous bromide hazardous waste into harmless end products, such as through acid-base neutralization, oxidation-reduction or precipitation.

[0007] 4. Recycling: Consider using appropriate technologies to recover valuable components from cuprous bromide hazardous waste to achieve resource recycling.

[0008] At present, there are no specific cases of cuprous bromide hazardous waste recycling in China, but scientific research institutions and environmental protection companies are researching and developing related technologies. Existing literature provides different methods for preparing copper powder, but does not consider the impact of other organic matter on copper powder, and does not achieve the recovery of bromine. Therefore, it is of great practical significance to develop an environmentally friendly and efficient method for treating cuprous bromide hazardous waste. Summary of the invention

[0009] In view of the above-mentioned shortcomings and deficiencies in the existing cuprous bromide hazardous waste recycling and treatment, the present invention provides a process for preparing sodium bromide using DMAC cuprous bromide hazardous waste.

[0010] The present invention utilizes DMAC cuprous bromide hazardous waste to prepare sodium bromide, which specifically comprises the following steps:

[0011] Step 1: Raw material preparation

[0012] Collect cuprous bromide hazardous waste (derived from but not limited to the residue produced by falling film evaporation of the filtrate after neutralization and precipitation filtration in the tetrafluorobutadiene production process after zincation, the copper content in the hazardous waste is about 15%, mainly in the form of cuprous (I) precipitation, and a small part in the form of copper (II), and the hazardous waste contains about 35% DMAC, so the hazardous waste is partially dissolved in water, but the aqueous solution still exists in the form of solid precipitation), and perform preliminary sorting on it to remove impurities and pollutants;

[0013] Step 2: Grinding and pretreatment

[0014] The cuprous bromide hazardous waste is ground and sieved, and then cleaned with 2-16% methanol-containing ethyl acetate cleaning solution; the ratio of hazardous waste to cleaning solution is 1:1-1:3, and the cleaning time is 30-150 minutes; after cleaning, the solid is stored for use in subsequent processes;

[0015] Step 3: Reduction reaction

[0016] Add the pretreated cuprous bromide hazardous waste solids into the reaction tank, disperse them in water at a ratio of 1:1, add the reducing agent after stirring for reaction, and the stirring speed is 200~1600rps; the reducing agent formula is zinc powder, aluminum powder or reducing iron powder, the reaction temperature is 80~90℃, and the reaction time is 1~8h; during the reaction, spray isomeric tridecanol, propylene glycol, n-butanol or phenylethanol dispersant (first, to make the copper powder production process uniform and control the particle size at the micron level, and second, to play a defoaming role);

[0017] Step 4: Separation and purification

[0018] After the reduction reaction is completed, the reaction product is separated from the unreacted substance by filtering or centrifuging to obtain a solution containing sodium bromide;

[0019] Step 5: Sodium bromide solution pretreatment

[0020] Pre-treat the sodium bromide solution by dichloromethane extraction or sodium hypochlorite oxidation to remove most of the residual organic matter;

[0021] Step 6: Preparation of Sodium Bromide

[0022] Bromine is prepared by electrolysis, separated by air stripping, absorbed by sodium hydroxide, reduced by urea to obtain sodium bromide mother liquor, and then dehydrated and dried to obtain sodium bromide crystals;

[0023] Step 7: Product Testing

[0024] The prepared sodium bromide is quality tested to ensure that the product meets relevant standards.

[0025] On the basis of the above technical solution, the present invention optimizes and defines the nodes and steps of the preparation process, specifically including the following three aspects:

[0026] 1. In the grinding and pretreatment of step 2, it is preferred to use 8% methanol-containing ethyl acetate cleaning solution to clean the cuprous bromide hazardous waste, the ratio of hazardous waste to cleaning solution is preferably 1:1~1:1.5, and the cleaning time is preferably 120 min.

[0027] 2. In the reduction reaction of step 3, zinc powder is used as the reducing agent; the stirring speed is preferably 1400-1600 rps; the reaction time is preferably 4 h; and 1-3% of isotridecyl alcohol is sprayed during the reaction.

[0028] 3. In the preparation of sodium bromide in step 6, the electrolysis process uses urea in an ion membrane electrolysis system; the amount of urea added is preferably 8-8.5%.

[0029] In addition, the present invention also provides the application of the preparation of sodium bromide: application in an organic solvent system of a halogen compound containing a catalytic metal; the catalytic metal includes nickel, copper, silver, gold, platinum or palladium.

[0030] Beneficial effects of the present invention:

[0031] The present invention uses an innovative process to prepare high-purity sodium bromide crystals from cuprous bromide hazardous waste, which can be used to prepare other bromine-containing compounds and has broad application prospects. At the same time, the use of cuprous bromide hazardous waste to prepare high-purity ultrafine copper powder realizes the resource utilization of hazardous waste, effectively solves the problem of environmental pollution, and creates significant economic value.

[0032] The present invention adopts an electrolytic method to prepare bromine, has simple equipment, is easy to operate, has high electrolysis efficiency, and has a bromine recovery rate of more than 99%. High-purity sodium bromide mother liquor is prepared by reducing sodium hypobromite in a solution with urea, and high-purity sodium bromide crystals are further prepared by dehydration and drying. The process operation is simple, the reaction efficiency is high, the prepared product has high purity, and the recovery rate is high.

[0033] In summary, the present invention not only improves the utilization rate of raw materials, but also realizes the efficient recovery of various substances, has good application prospects and promotion value, is suitable for treating organic solvent systems containing catalytic metal halogen compounds, and realizes the recovery of halogen elements and catalytic metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The present invention is a flow chart of the preparation process. DETAILED DESCRIPTION

[0035] In order to make the above and other purposes, features, and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with specific embodiments. The test materials, reagents, etc. used in the following examples can be obtained through commercial channels or known experimental methods.

[0036] The following are specific embodiments of the present invention, but are not limited thereto:

[0037] 1. Implementation methods of hazardous waste pretreatment:

[0038] 1.1. Choice of cleaning agent

[0039] The solvents that are more effective for dissolving DMAC are generally dichloromethane, ethyl acetate, methanol and acetone. Take 100g of solid waste (residue produced by falling film evaporation of the filtrate after zincification and precipitation filtration in the tetrafluorobutadiene production process), wash it with 1:1 pure solvent for 30 minutes, detect the bromine content in the liquid after washing and the DMAC content in the solid after washing, calculate the cuprous bromide loss rate and DMAC removal rate, and the washing effect is as follows:

[0040] Cleaning agent Dichloromethane Ethyl acetate Methanol acetone Cuprous bromide loss rate 41.34% 5.88% 37.52% 73.26% DMAC removal rate 77.59% 41.23% 94.31% 56.43% Difficulty of the process Volatile and difficult to clean Easy to clean Easier to clean Easy to clean

[0041] Dichloromethane and acetone have high cuprous bromide loss rates. Dichloromethane and acetone can be excluded according to actual conditions. Ethyl acetate and methanol need to be combined in proportion to achieve the maximum cleaning effect. According to the above experimental results, it is believed that ethyl acetate should be used as the base liquid. The effect of the amount of methanol added on the cleaning effect is as follows:

[0042] Methanol addition amount 2% 4% 6% 8% 10% 12% 14% 16% Cuprous bromide loss rate% 4.56 5.28 6.01 6.38 7.53 9.86 13.26 18.96 DMAC removal rate% 65.69 73.87 80.13 85.12 84.66 83.27 84.79 85.31

[0043] Through the above implementation, when the amount of methanol added reaches 8%, the removal rate of DMAC stabilizes at about 85%, but continued addition will lead to the loss of cuprous bromide, so the optimal addition amount is 8%.

[0044] 1.2.Choice of cleaning ratio

[0045] Different cleaning ratios have a great influence on the cleaning effect. Therefore, we designed cleaning ratios of 1:1, 1:1.5, 1:2, 1:2.5, and 1:3. The cleaning results after 30 minutes of cleaning with 8% methanol addition are as follows:

[0046] Cleaning ratio 1:1 1:1.5 1:2 1:2.5 1:3 Cuprous bromide loss rate% 6.42 7.38 11.67 18.92 24.44 DMAC removal rate% 85.49 90.31 92.27 93.14 94.26

[0047] As the cleaning ratio increases, the cuprous bromide loss rate increases rapidly, and the DMAC removal rate does not change significantly. Therefore, the greatest economic benefit is achieved under a 1:1.5 cleaning ratio.

[0048] 1.3.Choice of cleaning time

[0049] The cleaning time will affect the removal rate of DMAC, so we implemented cleaning for 30min, 60min, 90min, 120min, and 150min. The results of the addition of 8% methanol and a dosing ratio of 1:1.5 are as follows:

[0050] Cleaning time 30min 60min 90min 120min 150min Cuprous bromide loss rate% 7.53 7.66 7.78 7.75 8.02 DMAC removal rate% 90.26 92.55 94.18 96.47 95.83

[0051] Through the above implementation, the maximum DMAC removal rate and the lower cuprous bromide loss rate were achieved when the cleaning time was 120 min.

[0052] In summary, adding 8% ethyl acetate containing methanol as a cleaning agent and cleaning for 120 minutes at a cleaning ratio of 1:1.5 has the best effect on the pretreatment of hazardous waste.

[0053] 2. Reduction reaction

[0054] The reducing agents include metal reducing agents (zinc powder, aluminum powder, reducing iron powder), hydrazine hydrate, formaldehyde, etc.; the pretreated cuprous bromide hazardous waste solid is added to the reaction tank, dispersed in water at a ratio of 1:1, stirred and then added with the reducing agent for reaction, with a stirring speed of 200-1600rps; the reducing agent formula is zinc powder, aluminum powder or reducing iron powder, the reaction temperature is 80-90°C, and the reaction time is 1~8h; during the reaction, isomeric tridecanol, propylene glycol, n-butanol or phenylethanol dispersant is sprayed.

[0055] 3. Separation and purification implementation methods

[0056] After the reduction reaction is completed, the reaction product is separated from the unreacted substance by filtering or centrifuging to obtain a solution containing sodium bromide.

[0057] 4. Preparation method of sodium bromide

[0058] Due to the complex composition of the system, traditional extraction, concentration and crystallization, ion exchange and other methods cannot meet the actual requirements. We innovatively use electrolytic bromine extraction, combined with air stripping, to prepare to produce high-purity sodium bromide mother liquor, and then use the method of concentration into salt to produce high-purity sodium bromide.

[0059] Electrolysis principle: Anode reaction: 2Br - -e - =Br2

[0060] Cathode reaction: 2H + +e - =H2

[0061] The electrolysis process is carried out as follows:

[0062] An ion membrane electrolysis system is adopted, with the positive and negative chambers separated. Different solutions are respectively introduced into the positive and negative chambers to meet different needs. 15% hydrochloric acid is introduced into the cathode, and the pH change is monitored during the process. The pretreated sodium bromide solution is introduced into the anode, and the bromide ion content in the solution is monitored during the process. Under the action of a certain current and voltage, bromine is produced by electrolysis, which is separated by air stripping and absorbed by sodium hydroxide solution to obtain a sodium bromide solution. A certain amount of urea is added to reduce sodium hypobromite to sodium bromide to obtain a high-purity sodium bromide solution, which is then concentrated and dried to obtain high-purity sodium bromide crystals.

[0063] Electrolysis time and bromine content changes during electrolysis:

[0064] Electrolysis time / h 0 1 2 3 4 5 6 Electrolysis current / A 0 54.45 53.28 50.17 47.26 40.76 38.33 Cathode pH 0.6 0.8 1.1 1.5 1.9 2.3 2.8 Anode bromine content mg / L 32456 27572 21986 15098 9889 4322 315 CODmg / L 62471 57489 51453 45989 38233 31201 25442

[0065] The bromine electrolysis recovery rate is greater than 99%, the electrolysis effect is high, the structure is simple, the operation is simple, no other chemicals need to be added, and continuous operation is possible. The COD in the electrolysis process is continuously reduced until the bromine extraction is completed, and the COD removal rate reaches 59%.

[0066] The reaction principle of sodium hydroxide absorbing bromine: Br2+2NaOH=NaBr+NaBrO+H2O

[0067] Principle of urea reduction reaction: 3NaBrO+CO(NH2)2=3NaBr+CO2↑+N2↑+2H2O

[0068] The absorption process and pH changes are as follows:

[0069] Absorption time / h 0 1 2 3 4 5 6 pH 14 13.04 12.10 11.07 9.89 8.03 6.36

[0070] The absorption reaction speed of sodium hydroxide solution is fast and the absorption efficiency is high. The progress of the reaction can be known by monitoring the pH during the process.

[0071] After the sodium hydroxide solution has been absorbed, it is reduced with urea solution to obtain high-purity sodium bromide mother liquor. The mother liquor is sprayed into a hot air circulator to be dehydrated and dried into high-purity sodium bromide crystals.

[0072] The relationship between the amount of urea added and the purity of sodium bromide is as follows:

[0073] Urea addition amount / % 6 6.5 7 7.5 8 8.5 9 Sodium bromide purity / % 96.7 97.6 98.4 99.1 99.6 99.5 98.7

[0074] By adding 8%-8.5% urea, the sodium hypobromite in the solution can be effectively reduced, and more than 99.5% sodium bromide crystals can be prepared by drying and dehydration.

[0075] 5. Product quality

[0076] Sodium bromide:

[0077] Serial number project index 1 Sodium bromide content, w / % ≥99.50 2 Moisture, w / % ≤0.3 3 Bromate, w / % ≤0.003

[0078] The applicant declares that, based on the above embodiments, technicians in the relevant technical field combine the specific content point value of a component in the above embodiments with the technical solutions in the content of the invention to produce a new numerical range, which is also one of the recorded ranges of the present invention. In order to make the specification concise, the present application no longer lists these numerical ranges.

Claims

1. A process for preparing sodium bromide using DMAC cuprous bromide hazardous waste, characterized in that: The steps include: Step 1: Raw material preparation Collect cuprous bromide hazardous waste and conduct preliminary sorting to remove impurities and pollutants; Step 2: Grinding and pretreatment The cuprous bromide hazardous waste is ground and passed through a 60-mesh sieve, and is cleaned with a 2-16% special organic solvent cleaning solution containing methanol; the ratio of hazardous waste to cleaning solution is 1:1-1:3, and the cleaning time is 30-150 minutes; after cleaning, the solid is stored for use in subsequent processes; Step 3: Reduction reaction The pretreated cuprous bromide hazardous waste solid is added to the reaction tank, dispersed in water at a ratio of 1:1, stirred and then added with a reducing agent for reaction, with a stirring speed of 200-1600rps; the reducing agent formula is zinc powder, aluminum powder or reducing iron powder, the reaction temperature is 80-90°C, and the reaction time is 1-8h; during the reaction, an alcohol dispersant such as isotridecyl alcohol or phenylethyl alcohol is sprayed; Step 4: Separation and purification After the reduction reaction is completed, the reaction product is separated from the unreacted substances by filtering or centrifuging to obtain a solution containing sodium bromide; Step 5: Sodium bromide solution pretreatment Pre-treating the sodium bromide solution by extraction with halogenated hydrocarbons or oxidation with oxidants to remove most of the residual organic matter; Step 6: Preparation of Sodium Bromide Bromine is prepared by electrolysis, separated by air stripping, absorbed by sodium hydroxide, reduced by a reducing agent to obtain sodium bromide mother liquor, and then dehydrated and dried to obtain sodium bromide crystals; Step 7: Product Testing The prepared ultrafine copper powder is quality tested to ensure that the product meets relevant standards.

2. A process for preparing sodium bromide using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the grinding and pretreatment of step 2, 8% of a special organic solvent cleaning solution containing methanol is used to clean the cuprous bromide hazardous waste, the ratio of hazardous waste to cleaning solution is 1:1~1:1.5, and the cleaning time is 120 minutes.

3. A process for preparing sodium bromide using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the reduction reaction of step 3, zinc powder is used as the reducing agent; the stirring speed is 1400-1600 rps; the reaction time is 4 h; and 1-3% of isotridecyl alcohol is sprayed during the reaction.

4. A process for preparing sodium bromide using DMAC cuprous bromide hazardous waste as claimed in claim 1, characterized in that: In the preparation of sodium bromide in step 6, an ion membrane electrolysis system reducing agent is used in the electrolysis process; the amount of the reducing agent added is 8-8.5%.

5. The application of the sodium bromide process as claimed in claim 1, characterized in that: The preparation process is applied to an organic solvent system of a halogen compound containing a catalytic metal; the catalytic metal includes nickel, copper, silver, gold, platinum or palladium.