Method for circularly producing pseudo-boehmite under chromium salt production system

By adding acid to the aluminum-containing sodium chromate alkali solution in the chromium salt production system to generate aluminum sludge and reacting with sodium bicarbonate, combined with carbon separation and heat treatment technology, the problem of low aluminum resource utilization in chromium salt production is solved and achieved High-efficiency, low-consumption pseudo-boehmite preparation and resource recycling improve product performance.

CN118724036APending Publication Date: 2024-10-01SICHUAN YINHE CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410879328.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The utilization rate of aluminum resources in the by-products produced during the existing chromium salt production process is low, and the existing pseudo-boehmite preparation process equipment has large investments, high energy consumption, and poor environmental protection, making it difficult to meet the industrial needs of the chromium salt industry.

Method used

The aluminum-containing sodium chromate alkali solution produced in the chromium salt production system is added with acid to form aluminum sludge, which is reduced to aluminum liquid by adding alkali, reacts with a saturated solution of sodium bicarbonate to form pseudo-boehmite, and is recycled through a carbon separation reactor Sodium bicarbonate solution and solid are recycled, and at the same time, staged heat treatment and hole expansion treatment are performed to improve the performance of pseudo-boehmite.

Benefits of technology

It achieves efficient recycling of aluminum resources, generates pseudo-boehmite with stable performance, reduces equipment investment and energy consumption, and improves the recycling rate of aluminum resources and the pore volume and adsorption properties of pseudo-boehmite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724036A_ABST
    Figure CN118724036A_ABST
Patent Text Reader

Abstract

The invention discloses a method for cyclically producing pseudo-boehmite under a chromium salt production system. The method comprises the following steps: adding an acid into an aluminum-containing sodium chromate alkali liquor to adjust the pH value to generate aluminum mud; adding alkali into the aluminum mud, slurrying and reducing to generate molten aluminum; after being diluted, the molten aluminum reacts with a sodium bicarbonate solution to generate pseudo-boehmite and a sodium carbonate solution; transferring the sodium carbonate solution into a carbonation reactor, introducing CO2 to generate a sodium bicarbonate saturated solution and separate out a sodium bicarbonate solid, returning the sodium bicarbonate saturated solution to react with the diluted molten aluminum, and adding chromite into the sodium bicarbonate solid for co-baking to generate an aluminum-containing sodium chromate alkali solution and CO2. The method has the beneficial effects that the aluminum sludge is directly and continuously neutralized with the sodium bicarbonate saturated solution to generate the pseudo-boehmite, and the pseudo-boehmite with more stable performance can be generated; various substances in the production can be effectively recycled; in the aging process, the temperature is increased, ammonium bicarbonate is added to adjust the pH value, meanwhile, a pore-enlarging agent is added into the obtained pseudo-boehmite for segmented heat treatment, the pore volume of the pseudo-boehmite can be increased, and therefore the adsorbability of the pseudo-boehmite is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum extraction in chromium salt industry, and specifically relates to a method for producing pseudo-boehmite in a lower circulation manner in a chromium salt production system. Background Art

[0002] The aluminum-containing sodium chromate lye produced in the production process of chromium salts contains rich aluminum resources, but the utilization rate of this part of aluminum resources is currently low. At the same time, the production of chromium salts also produces a large amount of by-products such as sodium bicarbonate crude salt. How to improve the recovery rate and recycling degree of aluminum resources in these by-products has become one of the technical problems that the chromium salt industry must solve. There are many preparation methods for pseudo-boehmite in the industry, and technicians in this field have conducted multi-faceted research on pseudo-boehmite.

[0003] The existing preparation methods of pseudo-boehmite mainly rely on the alumina industry, and mostly adopt hydrothermal synthesis, organic solvent extraction and other process routes. These methods require large equipment investment, high energy consumption, poor environmental protection, and are not suitable for the application needs of the chromium salt industry.

[0004] Chinese patent CN117069131A uses a method of melting aluminum oxide with sodium hydroxide to prepare pseudo-boehmite. The main process includes filtration precipitation, hydrazine hydrate reduction, ammonium bicarbonate precipitation, multiple water washings, etc. This method has complex process steps and is difficult to adapt to large-scale industrial needs in the chromium salt industry.

[0005] Chinese patent CN115259189A uses industrial aluminum hydroxide as raw material, and utilizes hydrothermal reaction and multi-step treatment to produce pseudo-boehmite products. Hydrothermal conditions are conducive to sodium removal, and thermal treatment of ammonium aluminum carbonate can also obtain activated alumina. However, the entire process needs to be carried out under high temperature and high pressure conditions, so the equipment investment and energy consumption are relatively large.

[0006] Chinese patent CN109279634A uses the alkaline solution obtained after roasting chromite as raw material, and prepares pseudo-boehmite products through processes such as filtration, neutralization precipitation, gelation and drying. It is necessary to add reagents such as sulfuric acid and catalysts, which increases the cost investment.

[0007] Chromium salt production can obtain a large amount of aluminum resources, but they have not been effectively utilized for a long time. Therefore, it is urgent to develop a new pseudo-boehmite process that is suitable for the chromium salt process system and has high efficiency and low consumption. This is of great significance to the realization of aluminum resource utilization in chromium salt production. Summary of the invention

[0008] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0009] In order to achieve these purposes and other advantages of the present invention, a method for producing pseudo-boehmite in a chromium salt production system is provided, wherein an aluminum-containing sodium chromate alkali solution produced in the chromium salt production system is acidified to generate aluminum mud, and then an alkali is added to reduce it to aluminum liquid, and the aluminum liquid is reacted with a saturated sodium bicarbonate solution to obtain pseudo-boehmite, and the sodium carbonate solution generated in the reaction process is reacted with CO 2 Carbon separation is carried out in the carbon separation reactor, and the generated saturated sodium bicarbonate solution and precipitated sodium bicarbonate solid are returned to the chromium salt production system for recycling.

[0010] Preferably, the method comprises the following steps:

[0011] S1, adding acid to the alkali solution containing sodium chromate to adjust the pH, reacting to generate aluminum mud, and then adding alkali to the aluminum mud to reduce it to aluminum liquid;

[0012] S2, diluting the aluminum liquid in S1 and mixing it with a saturated sodium bicarbonate solution to obtain a suspension, and then aging it to generate pseudo-boehmite and a sodium carbonate solution;

[0013] S3, transfer the sodium carbonate solution obtained in S2 into the carbon fractionation reactor, and introduce CO 2 Afterwards, a saturated sodium bicarbonate solution is generated and sodium bicarbonate solid is precipitated, and the saturated sodium bicarbonate solution is returned to S2;

[0014] S4, adding the solid sodium bicarbonate precipitated in S3 to chromite for co-roasting to generate an alkali solution containing sodium aluminum chromate and CO 2 , containing sodium aluminum chromate alkali solution returned to S1, CO 2 Return to S3.

[0015] Preferably, in S1, the acid added is a carbonized liquid obtained by graded carbonization of a sodium chromate solution, the main component of which is Na 2 Cr 2 O 7 ·2H 2 O, acidic, containing sodium aluminum chromate alkali solution and carbonizing liquid in a mass ratio of 0.5-3:8-12.

[0016] Preferably, in S1, the reaction temperature after adding the acid is 70-90° C., and the end point pH is 6.5-8.

[0017] Preferably, in S1, the alkali added is sodium hydroxide, and the mass ratio of aluminum mud to alkali is 10-17:3-8.

[0018] Preferably, in S1, after adding the alkali, the reaction temperature is 60-100° C., and the insulation time is 0.5-3 h.

[0019] Preferably, in S2, the aluminum liquid is diluted to 20-50 g / L, and the flow rate ratio of the aluminum liquid to the saturated sodium bicarbonate solution is 1-6:15-25.

[0020] Preferably, in S2, the aging reaction temperature is 10-50° C., and the aging time is 1-3 h.

[0021] Preferably, in S3, CO 2 The flow rate is 1-6 L / min, and the pressure of the carbon fraction reactor is 0.5-2 MPa.

[0022] Preferably, in S4, the mass ratio of chromite to solid sodium bicarbonate is 8-13:1-3, and the roasting temperature is 800-1500°C.

[0023] In order to increase the pore volume of pseudo-boehmite and improve its performance, in S2, after obtaining the suspension, alkali is added to further adjust the pH to 9.8-10.5, and the aging temperature is increased to 70-100°C. The added alkali is at least one of ammonium bicarbonate, sodium carbonate and sodium hydroxide.

[0024] Preferably, the pseudo-boehmite obtained in S2 is subjected to a staged heat treatment by:

[0025] S21, placing the pseudo-boehmite into a heating furnace, slowly heating to 90-110° C., heating rate 2-5° C. / min, and keeping warm for 0.5-1 h;

[0026] S22, adding the pseudo-boehmite heat-treated in S21, the pore-enlarging agent, and deionized water into a hydrothermal reactor in a mass ratio of 1-1.5:0.5-1:8-10, and hydrothermally reacting at 120-160° C. for 6-8 hours, cooling, and filtering;

[0027] S23. Put the pseudo-boehmite after the hydrothermal reaction in S22 into the heating furnace again, slowly heat it to 350-450°C, with a heating rate of 5-10°C / min, keep it warm for 2-4 hours, and cool it to room temperature in the heating furnace.

[0028] Preferably, the pore expanding agent in S22 is at least one of polypropylene glycol, polybutylene glycol, polyvinyl alcohol, starch and cellulose.

[0029] The present invention has at least the following beneficial effects:

[0030] (1) The present invention adopts a method of directly neutralizing aluminum mud with a saturated sodium bicarbonate solution to generate pseudo-boehmite. Compared with strong acid, the weak acidity of sodium bicarbonate is relatively mild, and a pseudo-boehmite product with more stable performance can be generated;

[0031] (2) The source of the saturated sodium bicarbonate solution in the present invention is obtained by subjecting the sodium carbonate solution generated after continuous neutralization to a carbon fractionation process, which can effectively recover the sodium bicarbonate for the preparation of pseudo-boehmite;

[0032] (3) In the present invention, the sodium bicarbonate solid precipitated by the carbon separation method can be directly used for calcium-free roasting of chromite, thereby reducing the cost expenditure of purchasing sodium carbonate and sodium bicarbonate during the roasting process;

[0033] (4) The present invention uses the calcined CO 2 Carry out carbon fractionation treatment of chromium salt solution, completing the comprehensive utilization and circulation of resources in the whole process from chromium salt production to aluminum resource extraction and pseudo-boehmite preparation;

[0034] (5) In the present invention, ammonium bicarbonate is added during aging to further adjust the pH value, and the aging temperature is increased, so that the ammonium bicarbonate can be decomposed to generate gas, which is beneficial to increasing the pore volume of the pseudo-boehmite. At the same time, the generated gas overflows without introducing new impurities. The obtained pseudo-boehmite is subjected to segmented heat treatment and a pore expanding agent is added during the heat treatment process, which can also increase the pore volume of the pseudo-boehmite, thereby further improving its adsorption.

[0035] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a flow chart of Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0038] It should be understood that terms such as “having”, “including” and “comprising” used herein do not specify the existence or addition of one or more other elements or combinations thereof.

[0039] Example 1

[0040] like Figure 1 As shown, a method for producing pseudo-boehmite in a circulation system of a chromium salt production system comprises the following steps;

[0041] S1, aluminum content (in Al 2 O 3 2000mL of 40g / L sodium chromate alkali solution containing aluminum chromate was added to sodium chromate solution at 70°C for graded carbonization to obtain a carbonized liquid (prepared by the method of patent CN102649585A), the main component of which is Na 2 Cr 2 O 7 ·2H 2O, acidic, adjust pH to 6.5, filter to obtain aluminum mud, add the aluminum mud into 800mL of 150g / L sodium hydroxide solution, keep warm at 70℃ for 1h to generate aluminum liquid, the mass ratio of aluminum mud to sodium hydroxide in the solution is 13:6;

[0042] S2, dilute the aluminum liquid obtained from S2 to Al 2 O 3 The mass concentration is 30g / L, and then mixed with a saturated solution of sodium bicarbonate. The mixing is continuous neutralization. During mixing, a peristaltic pump is used to control the flow rate ratio of the aluminum liquid and the saturated solution of sodium bicarbonate to be 1L / min:10L / min. When the aluminum liquid is added, the mixing is stopped to obtain a suspension. The suspension is heated to 25°C, aged for 3h, and filtered to obtain pseudo-boehmite and sodium carbonate solution.

[0043] S3, the sodium carbonate solution obtained in S2 was transferred to the carbon fraction reactor, the pressure of the carbon fraction reactor was 1Mpa, and CO was introduced at a flow rate of 3L / min 2 Afterwards, a saturated sodium bicarbonate solution is generated and sodium bicarbonate solid is precipitated, and the saturated sodium bicarbonate solution is returned to S2 to react with aluminum liquid to achieve cyclic continuous production of pseudo-boehmite;

[0044] S4, adding the solid sodium bicarbonate precipitated in S3 to the chromite in a mass ratio of 8:1 and co-roasting at 850°C to generate an alkali solution containing sodium aluminum chromate and CO 2 The alkali solution containing sodium aluminum chromate is returned to S1 for recycling to extract aluminum, CO 2 Transfer to S3, and after reacting with the sodium carbonate solution in the carbon fraction reactor, a saturated sodium bicarbonate solution and sodium bicarbonate solid are formed again, thereby realizing the recycling of the components of the chromium salt production system.

[0045] The pseudo-boehmite obtained from S2 was sampled and tested. The peptization index of the pseudo-boehmite was 96% and the pore volume was 1.05 cm 3 / g.

[0046] Example 2

[0047] A method for producing pseudo-boehmite in a chromium salt production system in a downward cycle comprises the following steps:

[0048] S1, aluminum content (in Al 2 O 3 2000mL of 40g / L sodium chromate alkali solution containing aluminum chromate was added to sodium chromate solution at 75°C for graded carbonization to obtain a carbonized liquid (prepared by the method of patent CN102649585A), the main component of which is Na 2 Cr 2 O 7 ·2H 2O, acidic, adjust pH to 7.0, filter to obtain aluminum mud; add the aluminum mud into 700mL of 200g / L sodium hydroxide solution, keep warm at 75℃ for 2h to generate aluminum liquid, the mass ratio of aluminum mud to sodium hydroxide in the solution is 13:8;

[0049] S2, dilute the aluminum liquid obtained in S1 to Al 2 O 3 The mass concentration is 50g / L, and then mixed with a saturated sodium bicarbonate solution, and the mixing is continuous neutralization. During the mixing, a peristaltic pump is used to control the flow rate ratio of the aluminum liquid and the saturated sodium bicarbonate solution to be 1L / min:17L / min, until the aluminum liquid is added, the mixing is stopped to obtain a suspension, and the suspension is heated to 35°C, aged for 3h, and filtered to obtain pseudo-boehmite and sodium carbonate solution;

[0050] S3, the sodium carbonate solution obtained in S2 was transferred to the carbon fractionation reactor, and CO was introduced at a flow rate of 3 L / min. 2 Afterwards, a saturated sodium bicarbonate solution is generated and sodium bicarbonate solid is precipitated, and the saturated sodium bicarbonate solution is returned to S2 to react with aluminum liquid to achieve cyclic continuous production of pseudo-boehmite;

[0051] S4, adding the solid sodium bicarbonate precipitated in S3 to the chromite in a mass ratio of 8:1 and co-roasting at 850°C to generate an alkali solution containing sodium aluminum chromate and CO 2 The alkali solution containing sodium aluminum chromate is returned to S1 for recycling to extract aluminum, CO 2 Transfer to S3, and after reacting with the sodium carbonate solution in the carbon fraction reactor, form sodium bicarbonate solution and sodium bicarbonate solid again, so as to realize the recycling of the components of the chromium salt production system.

[0052] The pseudo-boehmite obtained from S2 was sampled and tested. The peptization index of the pseudo-boehmite was 98% and the pore volume was 1.12 cm 3 / g.

[0053] Example 3

[0054] The difference between this embodiment and embodiment 2 is that after obtaining the suspension in S2, ammonium bicarbonate is added to adjust the pH to 10, and then the suspension is heated to 75° C., reacted for 3 hours, filtered, and pseudo-boehmite and sodium carbonate solution are obtained, and then the pseudo-boehmite is subjected to staged heat treatment by the following method:

[0055] S21, placing the pseudo-boehmite into a heating furnace, slowly heating to 105°C, heating rate 5°C / min, and keeping warm for 1h;

[0056] S22, adding the pseudo-boehmite, polybutylene glycol and deionized water after the heat treatment in S21 into a hydrothermal reactor in a mass ratio of 1.5:0.5:10, hydrothermally reacting at 120° C. for 8 h, cooling and filtering;

[0057] S23. Put the pseudo-boehmite after the hydrothermal reaction in S22 into the heating furnace again, slowly heat it to 400°C, with a heating rate of 10°C / min, keep it warm for 4 hours, and cool it to room temperature in the heating furnace.

[0058] The obtained pseudo-boehmite was sampled and tested, and the pore volume was 2.02cm 3 / g.

[0059] Example 4

[0060] The difference between this embodiment and embodiment 2 is that after obtaining the suspension in S2, ammonium bicarbonate is added to adjust the pH to 10, and then the suspension is heated to 75° C., reacted for 3 hours, filtered, and pseudo-boehmite and sodium carbonate solution are obtained, and then the pseudo-boehmite is subjected to staged heat treatment by the following method:

[0061] S21, placing the pseudo-boehmite into a heating furnace, slowly heating to 110°C, heating rate 5°C / min, and keeping warm for 1h;

[0062] S22, adding the pseudo-boehmite, polybutylene glycol and deionized water after the heat treatment in S21 into a hydrothermal reactor in a mass ratio of 1.5:1:10, hydrothermally reacting at 120° C. for 8 h, cooling and filtering;

[0063] S23. Put the pseudo-boehmite after the hydrothermal reaction in S22 into the heating furnace again, slowly heat it to 450°C, with a heating rate of 10°C / min, keep it warm for 4 hours, and cool it to room temperature in the heating furnace.

[0064] The obtained pseudo-boehmite was sampled and tested, and the pore volume was 2.11cm 3 / g.

[0065] Comparative Example 1

[0066] The difference between this comparative example and Example 3 is that the method for heat treating pseudo-boehmite is: placing the pseudo-boehmite in a heating furnace, slowly heating it to 110°C, with a heating rate of 5°C / min, and keeping it warm for 1 hour; placing the heat-treated pseudo-boehmite in a heating furnace again, slowly heating it to 450°C, with a heating rate of 10°C / min, and keeping it warm for 4 hours, and then cooling it to room temperature in the heating furnace.

[0067] The obtained pseudo-boehmite was sampled and tested, and the pore volume was 1.30cm 3 / g.

[0068] Comparative Example 2

[0069] The difference between this comparative example and Example 3 is that the method for heat treating pseudo-boehmite is: adding pseudo-boehmite, polybutylene glycol and deionized water in a mass ratio of 1.5:0.5:10 into a hydrothermal reactor, hydrothermally reacting at 120°C for 8 hours, cooling and filtering; placing the pseudo-boehmite after the hydrothermal reaction into a heating furnace again, slowly heating to 450°C, with a heating rate of 10°C / min, keeping warm for 4 hours, and cooling to room temperature in the heating furnace.

[0070] The obtained pseudo-boehmite was sampled and tested, and the pore volume was 1.44cm 3 / g.

[0071] Comparative Example 3

[0072] The difference between this comparative example and Example 3 is that the method for heat treating pseudo-boehmite is: adding pseudo-boehmite, polybutylene glycol and deionized water in a mass ratio of 1.5:0.5:10 into a hydrothermal reactor, hydrothermally reacting at 120° C. for 8 hours, cooling, filtering and drying.

[0073] The obtained pseudo-boehmite was sampled and tested, and the pore volume was 1.41cm 3 / g.

[0074] Comparative Example 4

[0075] The difference between this comparative example and Example 3 is that the method for heat treating pseudo-boehmite is: placing the pseudo-boehmite in a heating furnace, slowly heating it to 110°C, with a heating rate of 5°C / min, and keeping it warm for 1 hour; adding the heat-treated pseudo-boehmite, polybutylene glycol, and deionized water into a hydrothermal reactor in a mass ratio of 1.5:0.5:10, hydrothermally reacting at 120°C for 8 hours, cooling, and filtering.

[0076] The obtained pseudo-boehmite was sampled and tested, and the pore volume was 1.40cm 3 / g.

[0077] It can be seen from the sampling test results of Examples 1 to 4 and Comparative Examples 1 to 4 that the peptization index and pore volume of the pseudo-boehmite prepared by the present invention are large, indicating that the performance of the pseudo-boehmite is good. Adding ammonium bicarbonate during aging and increasing the aging temperature can further improve the performance of the prepared pseudo-boehmite; further performing segmented heat treatment on the pseudo-boehmite and using a pore expanding agent to expand the pores can effectively increase the pore volume of the pseudo-boehmite, thereby improving the performance of the pseudo-boehmite.

[0078] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for producing pseudo-boehmite in a chromium salt production system in a cycle, characterized in that: Acid is added to the aluminum-containing sodium chromate alkali solution produced in the chromium salt production system to generate aluminum mud, and then alkali is added to reduce it to aluminum liquid. The aluminum liquid reacts with a saturated sodium bicarbonate solution to obtain pseudo-boehmite, and the sodium carbonate solution generated in the reaction process is carbon-separated with CO2 in a carbon separation reactor, and the generated saturated sodium bicarbonate solution and the precipitated sodium bicarbonate solid are returned to the chromium salt production system for recycling.

2. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 1, characterized in that: The following steps are involved: S1, adding acid to the alkali solution containing sodium chromate to adjust the pH, reacting to generate aluminum mud, and then adding alkali to the aluminum mud to reduce it to aluminum liquid; S2, diluting the aluminum liquid in S1 and mixing it with a saturated sodium bicarbonate solution to obtain a suspension, and then aging it to generate pseudo-boehmite and a sodium carbonate solution; S3, the sodium carbonate solution obtained in S2 is transferred to the carbon fractionation reactor, after CO2 is introduced, a saturated sodium bicarbonate solution is generated and sodium bicarbonate solid is precipitated, and the saturated sodium bicarbonate solution is returned to S2; S4. The solid sodium bicarbonate precipitated in S3 is added to the chromite for co-roasting to generate an alkali solution containing sodium aluminum chromate and CO2. The alkali solution containing sodium aluminum chromate is returned to S1, and the CO2 is returned to S3.

3. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 2, characterized in that: In the S1, the added acid is a carbonized liquid obtained by graded carbonization of a sodium chromate solution, the main component of which is Na2Cr2O7·2H2O, which is acidic, and the mass ratio of the sodium aluminum chromate alkali solution to the carbonized liquid is 0.5-3:8-12.

4. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 2, characterized in that: In S1, after adding acid, the reaction temperature is 70-90° C., and the end point pH is 6.5-8.

5. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 2, characterized in that: In the S1, the added alkali is sodium hydroxide, and the mass ratio of aluminum mud to alkali is 10-17:3-8.

6. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 2, characterized in that: In S1, after adding the alkali, the reaction temperature is 60-100° C., and the insulation time is 0.5-3 h.

7. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 2, characterized in that: In S2, the aluminum liquid is diluted to 20-50 g / L, and the flow rate ratio of the aluminum liquid to the saturated sodium bicarbonate solution is 1-6:15-25.

8. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 2, characterized in that: In S2, the aging reaction temperature is 10-50° C., and the aging time is 1-3 hours.

9. The method for producing pseudo-boehmite by lower circulation in a chromium salt production system according to claim 2, characterized in that: In S3, the CO2 flow rate is 1-6 L / min, and the carbon fraction reactor pressure is 0.5-2 MPa.

10. The method for producing pseudo-boehmite in a lower circulation in a chromium salt production system according to claim 2, characterized in that: In the S4, the mass ratio of chromite to solid sodium bicarbonate is 8-13:1-3, and the roasting temperature is 800-1500°C.