Preparation method of lithium-doped low-nickel quaternary sodium ion battery positive electrode material
By doping lithium elements and reducing the nickel content in the sodium-ion battery cathode material, combined with sand spraying and high-temperature sintering processes, the structural instability problem caused by the reduced nickel content is solved, the capacity and rate performance of the battery are improved, and the cost is achieved reduction and safety performance improvement.
Patent Information
- Application Number
- CN202410956799.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing sodium-ion battery cathode materials to maintain electrochemical performance when reducing the nickel content, and reducing the nickel content will lead to structural instability and affect the cycle life and safety performance of the material.
By doping lithium with a smaller atomic radius to reduce the nickel content, and stabilizing the crystal lattice of the layered oxygen cathode material through the sand spray process and high-temperature sintering, combined with coating agent treatment, a high-capacity lithium-doped low-voltage Nickel quaternary sodium ion battery cathode material.
It significantly improves the specific capacity and rate performance of sodium-ion batteries, reduces raw material costs, enhances the stability and safety performance of materials, extends the cycle life of batteries, and simplifies the production process.
Smart Images

Figure CN118724083A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material, belonging to the technical field of sodium ion batteries. Background Art
[0002] In recent years, with the increasing consumption of non-renewable energy such as oil and coal, the environmental problems it brings are becoming increasingly severe. It is urgent to develop clean and efficient renewable energy. At present, lithium-ion batteries have occupied a place in the new energy industry due to their green environmental protection and high energy conversion efficiency. However, with the development of the economy, limited lithium resources cannot meet people's growing needs, and it is urgent to find products to replace lithium-ion batteries. Sodium and lithium are in the same family. Not only do they have similar physical and chemical properties, but the abundance of sodium resources is much higher than that of lithium. Even in terms of cost and safety, sodium has more advantages and is expected to be used in the field of large-scale energy storage.
[0003] The positive electrode materials of sodium ion batteries are mainly divided into layered oxygen transition metal oxides, Prussian blue and polyanion materials. Layered oxygen materials have attracted widespread attention due to their high specific capacity. At present, in order to obtain positive electrode materials for sodium ion batteries with higher specific capacity, the research and development of medium- and high-nickel transition metal oxides is mainly carried out. How to reduce the nickel content while maintaining the electrochemical properties has become a technical difficulty (which can reduce costs). Usually, the structure can be stabilized by doping inactive elements such as Mg, Zn, Cu, or coating the surface of the material with metal oxides such as ZrO2, TiO2, Al2O3, etc., to improve the capacity retention rate and promote long-term cyclability. Summary of the invention
[0004] The present invention aims at a method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material, which reduces the nickel content by doping lithium elements with a smaller atomic radius, stabilizes the lattice of the layered oxygen positive electrode material, makes the structure of the material more stable, and reduces the cost required on the raw material side. The prepared sodium ion battery positive electrode material has better specific capacity and rate performance, low residual alkali, higher compaction density, and has broad application prospects. The method specifically comprises the following steps:
[0005] A method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material, the specific steps are as follows:
[0006] (1) Weighing an iron source, a nickel source, and a manganese source, and placing them in a mixing chamber, adding an appropriate amount of solvent and stirring evenly, then adding a lithium source and a sodium source, stirring evenly, and passing them into a sand mill for sand grinding. After sand grinding for several hours, a uniformly mixed slurry is obtained;
[0007] (2) passing the mixed slurry into a spray dryer, wherein the peristaltic pump speed of the spray dryer is 20-50 r / min, the air inlet temperature is 200-220° C., the air outlet temperature is 100-120° C., and the air compressor frequency is 40-55 Hz, so as to control the particle size of the obtained precursor;
[0008] (3) The precursor obtained by spraying is placed in a sintering furnace into which gas is introduced and sintered for several hours. The obtained sample is crushed and sieved, and then placed in a ball mill, and a solvent and a coating agent are added for secondary mixing;
[0009] (4) After drying, the mixed sample is placed in a sintering furnace with protective gas for secondary calcination, and then crushed and sieved to obtain a sodium ion positive electrode material;
[0010] The structural formula of the obtained sodium ion positive electrode material is NaNi a Fe b Mn c Li d O2, where a+b+c+d=1, 0.1≤a≤0.15, 0.3≤b≤0.45, 0.4≤c≤0.5, a:b:c=15:40:45, 0.01≤d≤0.1.
[0011] The nickel source in step (1) is one or both of nickelous oxide and nickelous hydroxide, the manganese source is one or more of manganese tetraoxide, manganese trioxide, manganese hydroxide or manganese carbonate, and the iron source is one or both of ferric oxide and ferric hydroxide.
[0012] In step (1), the nickel source, iron source and manganese source are mixed in a molar ratio of 15:40:45, the lithium source: nickel iron manganese are mixed in a molar ratio of (0.01-0.1):1, and the sodium source: lithium nickel iron manganese are mixed in a molar ratio of (0.9-1.05):1.
[0013] The lithium salt in step (1) is lithium carbonate or lithium hydroxide, and the sodium source is sodium carbonate.
[0014] In step (1), the stirring speed is 80-120 r / min, the sand mill speed is 1200-1500 r / min, the sand mill power is 40-50 Hz, and the sand milling time is 0.5-4 h.
[0015] In step (3), the gas introduced is air or oxygen, the sintering temperature is 800-1000° C., the heating rate is 2-5° C. / min, and the insulation time is 12-15h.
[0016] The coating agent in step (3) is one or more of glucose, citric acid, polytetrafluoroethylene, phenolic resin, titanium oxide, aluminum oxide, zirconium oxide, etc.
[0017] The protective gas in step (4) is nitrogen or argon, the sintering temperature is 600-1000° C., and the insulation time is 4-8 hours.
[0018] The present invention mainly includes the following steps: after insoluble nickel, iron, manganese and other salts or oxides are mixed uniformly in a certain proportion, a certain amount of sodium salt and lithium salt are added, and after being fully mixed uniformly by means of sand milling spray and the like, a small amount of carbon source is pre-coated after high temperature sintering, post-treatment and the like, and a high-capacity lithium-doped low-nickel quaternary sodium ion battery positive electrode material is obtained after two sintering. The doped positive electrode material prepared by the present invention has the characteristics of compact surface morphology and uniform distribution. The process is not only simple in synthesis process, but also low in nickel content, which not only reduces the cost, but also further stabilizes the internal structure of the material after lithium doping, and the capacity and rate performance of the sodium ion battery obtained after sintering are also significantly improved, and has better safety performance and application prospects.
[0019] The present invention aims at providing a method for preparing a layered positive electrode material for a sodium ion battery at a low temperature, and reduces the material production cost by reducing the nickel content. However, the reduction of the nickel content will reduce the stability of the material, and enhance the Jahn-Teller effect generated by the charging and discharging process of the Mn-based material, resulting in the structure being often distorted and deformed. By doping a certain amount of lithium ions, the lattice structure of the material can be optimized, the stability of the material can be improved, and more sodium ions can be promoted to be deintercalated during the charging and discharging process, thereby improving the capacity and rate performance of the positive electrode material; in addition, by coating modification, the volume expansion and SEI film formation generated by the positive electrode material during the charging and discharging process can be effectively suppressed, and the cycle life of the battery is effectively improved; the preparation method of the present invention is simple, low-cost, the obtained positive electrode material is densely arranged, the particles are uniform, and the elements are evenly distributed, which is conducive to large-scale production and has broad application prospects in the field of large-scale energy storage. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a scanning electron microscope photo of the nickel iron manganese lithium sodium positive electrode material of Example 1
[0021] Figure 2 The first cycle voltage capacity curve of the nickel iron manganese sodium lithium oxide positive electrode material of Example 1
[0022] Figure 3 The charge and discharge curves of the first 50 cycles of the nickel iron manganese lithium sodium positive electrode material of Example 1 Specific implementation methods
[0024] The present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the described contents.
[0025] Example 1
[0026] A method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material specifically comprises the following steps:
[0027] (1) Ferrous oxide, nickelous oxide and manganese oxide are weighed in a molar ratio of 10:40:45 and placed in a mixing bin. An appropriate amount of pure water is added for stirring. Subsequently, a certain amount of lithium carbonate is weighed in a molar ratio of NFM:Li=1:0.055 and placed in the mixing bin for stirring. Sodium carbonate is weighed in a molar ratio of NFML:Na=1:0.95. After being stirred evenly, the mixture is passed into a sand mill for sand grinding for 1.5 hours to obtain a uniformly mixed slurry.
[0028] (2) The mixed slurry is passed into a spray dryer with a peristaltic pump speed of 25 r / min, an air inlet temperature of 220° C., an air outlet temperature of 110° C., and an air compressor power of 45 Hz. After a spraying time of 2 hours, a uniformly mixed precursor is obtained.
[0029] (3) The precursor obtained by spraying is placed in a sintering furnace into which air is introduced, and the temperature is increased to 950°C at a heating rate of 2°C / min and kept at this temperature for 15 hours. The obtained sample is crushed and sieved, and then placed in a ball mill. Alcohol is used as a solvent, and the positive electrode material and zirconium dioxide are mixed for a second time at a mass ratio of 1000:5.
[0030] (4) After the mixed sample is dried, it is placed in a sintering furnace protected by nitrogen and heated to 800° C. for 8 hours. After that, it is crushed and sieved to obtain a sodium ion positive electrode material.
[0031] Comparative Example 1
[0032] A method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material specifically comprises the following steps:
[0033] (1) Ferrous oxide, nickelous oxide and manganese oxide in a molar ratio of 10:40:45 are weighed and placed in a mixing bin, and an appropriate amount of pure water is added for stirring. Sodium carbonate is weighed in a molar ratio of NFM:Na=1:0.95, and after being stirred evenly, it is passed into a sand mill for sand grinding for 1.5 hours to obtain a uniformly mixed slurry.
[0034] (2) The mixed slurry is passed into a spray dryer with a peristaltic pump speed of 25 r / min, an air inlet temperature of 220° C., an air outlet temperature of 110° C., and an air compressor power of 45 Hz. After a spraying time of 2 hours, a uniformly mixed precursor is obtained.
[0035] (3) The precursor obtained by spraying is placed in a sintering furnace with air, and the temperature is increased to 950°C at a heating rate of 2°C / min. After being kept warm for 15 hours, the obtained sample is crushed and sieved, and then placed in a ball mill. Alcohol is used as a solvent, and the positive electrode material and zirconium dioxide are mixed again at a mass ratio of 1000:5.
[0036] (4) After the mixed sample is dried, it is placed in a sintering furnace protected by nitrogen and heated to 800° C. for 8 hours. After that, it is crushed and sieved to obtain a sodium ion positive electrode material.
[0037] Example 2
[0038] A method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material specifically comprises the following steps:
[0039] (1) Ferrous oxide, nickelous oxide and manganese oxide are weighed in a molar ratio of 10:40:45 and placed in a mixing bin, and an appropriate amount of pure water is added for stirring. Subsequently, a certain amount of lithium carbonate is weighed in a molar ratio of NFM:Li=1:0.02 and placed in the mixing bin for stirring. Sodium carbonate is weighed in a molar ratio of NFML:Na=1:1. After being stirred evenly, the mixture is passed into a sand mill for sand grinding for 2 hours to obtain a uniformly mixed slurry.
[0040] (2) The mixed slurry was introduced into a spray dryer with a peristaltic pump speed of 30 r / min, an air inlet temperature of 200°C, an air outlet temperature of 105°C, an air compressor power of 50 Hz, and a spray time of 1.5 hours to obtain a uniformly mixed precursor.
[0041] (3) The precursor obtained by spraying is placed in a sintering furnace with air, and the temperature is increased to 1000°C at a heating rate of 2°C / min. After being kept at this temperature for 12 hours, the obtained sample is crushed and sieved, and then placed in a ball mill. Alcohol is used as a solvent, and the positive electrode material and titanium dioxide are mixed again at a mass ratio of 1000:2.
[0042] (4) After the mixed sample is dried, it is placed in a sintering furnace protected by nitrogen and heated to 600° C. for 10 hours. After that, it is crushed and sieved to obtain a sodium ion positive electrode material.
[0043] Example 3
[0044] A method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material specifically comprises the following steps:
[0045] (1) Ferrous oxide, nickelous oxide and manganese oxide are weighed in a molar ratio of 10:40:45 and placed in a mixing bin. An appropriate amount of pure water is added for stirring. Subsequently, a certain amount of lithium carbonate is weighed in a molar ratio of NFM:Li=1:0.05 and placed in the mixing bin for stirring. Sodium carbonate is weighed in a molar ratio of NFML:Na=1:0.97. After being stirred evenly, the mixture is passed into a sand mill for sand grinding for 1.5 hours to obtain a uniformly mixed slurry.
[0046] (2) The mixed slurry was introduced into a spray dryer with a peristaltic pump speed of 20 r / min, an air inlet temperature of 210° C., an air outlet temperature of 115° C., and an air compressor power of 40 Hz. After a spraying time of 2 hours, a uniformly mixed precursor was obtained.
[0047] (3) The precursor obtained by spraying was placed in a sintering furnace with air, and the temperature was raised to 900°C at a heating rate of 5°C / min. After being kept at this temperature for 15 hours, the obtained sample was crushed and sieved, and then placed in a ball mill. Alcohol was used as a solvent, and the positive electrode material and glucose were mixed again at a mass ratio of 1000:5.
[0048] (4) After the mixed sample is dried, it is placed in a sintering furnace protected by nitrogen and heated to 700° C. for 5 hours. After that, it is crushed and sieved to obtain a sodium ion positive electrode material.
[0049] Example 4
[0050] (1) Ferrous oxide, nickelous oxide and manganese oxide are weighed in a molar ratio of 10:40:45 and placed in a mixing bin, and an appropriate amount of pure water is added for stirring. Subsequently, a certain amount of lithium carbonate is weighed in a molar ratio of NFM:Li=1:0.07 and placed in the mixing bin for stirring. Sodium carbonate is weighed in a molar ratio of NFML:Na=1:1.05. After being stirred evenly, the mixture is passed into a sand mill for sand grinding for 1 hour to obtain a uniformly mixed slurry.
[0051] (2) The mixed slurry was introduced into a spray dryer with a peristaltic pump speed of 25 r / min, an air inlet temperature of 200°C, an air outlet temperature of 110°C, an air compressor power of 45 Hz, and a spray time of 1.5 hours to obtain a uniformly mixed precursor.
[0052] (3) The precursor obtained by spraying was placed in a sintering furnace with air, and the temperature was raised to 950°C at a heating rate of 5°C / min. After being kept warm for 15 hours, the obtained sample was crushed and sieved, and then placed in a ball mill. Alcohol was used as a solvent, and the positive electrode material and phenolic resin were mixed again at a mass ratio of 1000:4.
[0053] (4) After the mixed sample is dried, it is placed in a nitrogen-protected sintering furnace and heated to 650° C. for 6 hours. After that, it is crushed and sieved to obtain a sodium ion positive electrode material.
[0054] Example 5
[0055] A method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material specifically comprises the following steps:
[0056] (1) Ferrous oxide, nickelous oxide and manganese oxide are weighed in a molar ratio of 10:40:45 and placed in a mixing bin. An appropriate amount of pure water is added for stirring. Subsequently, a certain amount of lithium carbonate is weighed in a molar ratio of NFM:Li=1:0.1 and placed in the mixing bin for stirring. Sodium carbonate is weighed in a molar ratio of NFML:Na=1:1.03. After being stirred evenly, the mixture is passed into a sand mill for sand grinding for 1.5 hours to obtain a uniformly mixed slurry.
[0057] (2) The mixed slurry was introduced into a spray dryer with a peristaltic pump speed of 30 r / min, an air inlet temperature of 210°C, an air outlet temperature of 105°C, an air compressor power of 45 Hz, and a spray time of 2 hours to obtain a uniformly mixed precursor.
[0058] (3) The precursor obtained by spraying is placed in a sintering furnace with air, and the temperature is raised to 980°C at a heating rate of 2°C / min. After being kept warm for 12 hours, the obtained sample is crushed and sieved, and then placed in a ball mill. The positive electrode material and aluminum oxide are mixed again at a mass ratio of 1000:3 using alcohol as a solvent.
[0059] (4) After the mixed sample is dried, it is placed in a nitrogen-protected sintering furnace and heated to 650° C. for 6 hours. After that, it is crushed and sieved to obtain a sodium ion positive electrode material.
[0060] Comparison of Examples
[0061] In the comparative example, nickel-iron-manganese quaternary positive electrode materials prepared with different lithium ratios were compared. The performance of the assembled batteries is shown in Table 1 below:
[0062] Table 1 Main parameters and sodium ion battery performance of Examples 1-5 and Comparative Example 1
[0063]
[0064] In addition, the above is only a preferred specific embodiment, but the protection scope of the present invention is not limited to this. Any technical personnel in this field can make some modifications and improvements within the technical scope disclosed by the present invention. Therefore, the protection scope of the present invention shall be based on the definition of the claims.
Claims
1. A method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material, characterized in that: The specific steps are as follows: (1) Weighing an iron source, a nickel source, and a manganese source, and placing them in a mixing chamber, adding an appropriate amount of solvent and stirring evenly, then adding a lithium source and a sodium source, stirring evenly, and passing them into a sand mill for sand grinding. After sand grinding for several hours, a uniformly mixed slurry is obtained; (2) passing the mixed slurry into a spray dryer, wherein the peristaltic pump speed of the spray dryer is 20-50 r / min, the air inlet temperature is 200-220° C., the air outlet temperature is 100-120° C., and the air compressor frequency is 40-55 Hz, so as to control the particle size of the obtained precursor; (3) The precursor obtained by spraying is placed in a sintering furnace into which gas is introduced and sintered for several hours. The obtained sample is crushed and sieved, and then placed in a ball mill, and a solvent and a coating agent are added for secondary mixing; (4) After drying, the mixed sample is placed in a sintering furnace with a protective gas for secondary calcination, and then crushed and sieved to obtain a sodium ion positive electrode material; The structural formula of the obtained sodium ion positive electrode material is NaNi a Fe b Mn c Li d O2, where a+b+c+d=1, 0.1≤a≤0.15, 0.3≤b≤0.45, 0.4≤c≤0.5, a:b:c=15:40:45, 0.01≤d≤0.
1.
2. The method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material according to claim 1, characterized in that: The nickel source in step (1) is one or both of nickelous oxide and nickelous hydroxide, the manganese source is one or more of manganese tetraoxide, manganese trioxide, manganese hydroxide or manganese carbonate, and the iron source is one or both of ferric oxide and ferric hydroxide.
3. The method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material according to claim 1, characterized in that: In step (1), the nickel source, iron source and manganese source are mixed in a molar ratio of 15:40:45, the lithium source: nickel iron manganese are mixed in a molar ratio of (0.01-0.1):1, and the sodium source: lithium nickel iron manganese are mixed in a molar ratio of (0.9-1.05):
1.
4. The method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material according to claim 1, characterized in that: The lithium salt in step (1) is lithium carbonate or lithium hydroxide, and the sodium source is sodium carbonate.
5. The method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material according to claim 1, characterized in that: In step (1), the stirring speed is 80-120 r / min, the sand mill speed is 1200-1500 r / min, the sand mill power is 40-50 Hz, and the sand milling time is 0.5-4 h.
6. The method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material according to claim 1, characterized in that: In step (3), the gas introduced is air or oxygen, the sintering temperature is 800-1000° C., the heating rate is 2-5° C. / min, and the insulation time is 12-15h.
7. The method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material according to claim 1, characterized in that: The coating agent in step (3) is one or more of glucose, citric acid, polytetrafluoroethylene, phenolic resin, titanium oxide, aluminum oxide, zirconium oxide, etc.
8. The method for preparing a lithium-doped low-nickel quaternary sodium ion battery positive electrode material according to claim 1, characterized in that: The protective gas in step (4) is nitrogen or argon, the sintering temperature is 600-1000° C., and the insulation time is 4-8 hours.