Preparation method and application of wet grinding silicon doped zero-valent iron composite material

By preparing wet-grinding silicon-doped zero-valent iron composite materials and using mechanochemical effects to generate polymers, the problem of insufficient degradation of chlorine-containing organic pollutants by zero-valent iron in the existing technology has been solved, and a high-efficiency, low-cost, and Environmentally friendly pollutant removal effect.

CN118724237APending Publication Date: 2024-10-01SHANGHAI JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410903293.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, zero-valent iron has limited ability to degrade chlorine-containing organic pollutants, and the modification method is costly and not environmentally friendly.

Method used

The preparation method of wet-grinding silicon-doped zero-valent iron composite materials is used. By mechanical ball milling silicic acid powder and zero-valent iron powder in anaerobic water, the polymer is generated by mechanochemical action to improve its resistance to chlorine-containing organic pollutants. Remove ability.

Benefits of technology

The removal effect of different chlorinated organic pollutants is significantly enhanced, the raw materials are widely used, the price is low, the preparation process has no waste water and waste, the operation is simple, and it has significant economic, environmental and social effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724237A_ABST
    Figure CN118724237A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of environmental chemistry, and particularly relates to a preparation method and application of a wet-ground silicon-doped zero-valent iron composite material, specifically, silicic acid powder and iron powder are mixed, a certain amount of oxygen-free water is added, then wet grinding is performed in an inert gas atmosphere or a vacuum environment, and the wet-ground silicon-doped zero-valent iron composite material can be prepared. The material can be used as a filling medium of an underground water permeable reactive barrier, and is suitable for repairing a polluted water body containing chlorine organic pollutants. The synthetic method disclosed by the invention is simple, wide in raw material source, low in price, low in dosage, safe to use, high in practicability, mild in reaction condition, easy to construct and operate, free of too high requirements on equipment, beneficial to large-scale popularization and remarkable in economic, environmental and social effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental chemistry, and in particular relates to a preparation method and application of a wet-ground silicon-doped zero-valent iron composite material. Background Art

[0002] Chlorinated pollutants are common groundwater contaminants in various regions. Due to their high volatility and toxicity, their transport, fate, and remediation in the subsurface have been intensively studied, especially biological and chemical dechlorination processes under anoxic conditions.

[0003] As early as the 1980s, zero-valent metal materials were used to remove chlorine-containing pollutants from the environment. It was not until the 1990s that iron was used as a treatment agent for the degradation of chlorine-containing pollutants. ZVI has attracted great interest because of its higher reactivity with TCE than natural minerals (such as mikanisite). Zero-valent iron (ZVI) is a green and environmentally friendly material with the characteristics of abundant sources, low price, strong metal activity and strong reducibility. It usually exists in the form of a core-shell structure, and its outer shell is composed of various iron oxides or hydrated oxides (referred to as iron oxide layer). However, zero-valent iron has the disadvantages of easy passivation, low reactivity, poor selectivity for certain pollutants, and easy production of by-products, so the selectivity and reduction ability of ZVI particles are low. Modification of surface functional species is a promising method to optimize ZVI, and efforts are still needed to find more affordable and greener processes.

[0004] Adding Si element is an effective modification method, which can adjust the interface adsorption and redox properties of magnetic particles and is widely used in materials and catalysis related fields. However, in the existing technology, silicate modification cannot significantly improve the degradation ability of silicon-doped zero-valent iron composite materials on chlorine-containing pollutants. Summary of the invention

[0005] In view of the limitations of the prior art for the modification and application of zero-valent iron, the present invention provides a method and application of wet-grinding silicon-doped zero-valent iron composite materials. The method is based on the principle of mechanochemistry, and utilizes mechanical shear force, impact force, friction force and other forces, and utilizes silicic acid and oxygen-free water to mechanically ball-mill the zero-valent iron to improve the removal ability of zero-valent iron for chlorine-containing organic pollutants. The specific technical scheme is as follows:

[0006] In a first aspect, the present invention provides a method for preparing a wet-ground silicon-doped zero-valent iron composite material, specifically comprising: mixing silicic acid powder and zero-valent iron powder, adding oxygen-free water, and ball milling in an inert gas atmosphere or a vacuum environment to obtain a wet-ground silicon-doped zero-valent iron composite material.

[0007] In the present invention, after a certain amount of oxygen-free water is added to the mixture of silicic acid powder and zero-valent iron powder, the silicic acid first reacts with the oxygen-free water to generate a silicic acid solution, and the silicic acid solution interacts with iron under the action of mechanochemistry to generate a series of polymers, namely, wet-ground silicon-doped zero-valent iron composite materials. Experimental verification shows that the obtained wet-ground silicon-doped zero-valent iron composite materials have significantly enhanced degradation capabilities for chlorine-containing organic pollutants.

[0008] Furthermore, the oxygen-free water is deionized water obtained by removing oxygen through nitrogen purging.

[0009] Furthermore, the molar ratio of the silicic acid to the zero-valent iron powder is 0.01 to 0.05.

[0010] Furthermore, the mass volume ratio of the zero-valent iron powder to oxygen-free water is 1 g: 25-30 μL.

[0011] Furthermore, the mass volume ratio of the zero-valent iron powder to oxygen-free water is 1 g:28 μL.

[0012] Furthermore, the mass volume ratio of the mixture of silicic acid and zero-valent iron powder to oxygen-free water is 0.030-0.040 g / μL.

[0013] Furthermore, the zero-valent iron powder is elemental iron powder, reduced iron powder, cast iron powder, pig iron powder or industrial scrap iron containing zero-valent iron, and the particle size of the reduced iron powder material is 2 to 30 μm.

[0014] Furthermore, the ball milling operation is: using a planetary ball mill for ball milling, the ball milling speed is 300 to 500 rpm, and the ball milling time is 2 to 30 hours.

[0015] Furthermore, sodium silicate powder and iron powder are mixed in proportion and then placed in a ball milling jar of a planetary ball mill for ball milling, wherein the ball milling jar is filled with zirconium oxide beads, and the filling amount of the ball milling medium is 8-20% of the volume of the ball milling jar cavity, wherein the diameter of the zirconium oxide beads is 6 mm.

[0016] In a second aspect, the present invention provides a wet-ground silicon-doped zero-valent iron composite material prepared by the above preparation method.

[0017] In a third aspect, the present invention provides an application of a wet-ground silicon-doped zero-valent iron composite material prepared by the above-mentioned preparation method in the repair of polluted water bodies containing chlorine-containing organic pollutants.

[0018] Furthermore, the chlorine-containing organic pollutant is at least one of trichloromethane (CF), trichloroethylene (TCE), 1,1-dichloroethylene (1,1-DCE) and trans-1,2-dichloroethylene (trans-1,2-DCE).

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The wet-ground silicon-doped zero-valent iron composite material synthesized by the method of the present invention has better removal effect on different chlorinated organic pollutants than the unmodified wet-ground silicon-doped zero-valent iron composite material.

[0021] (2) The raw materials used in the method of the present invention are widely available, inexpensive, and used in low amounts. No wastewater or waste is generated during the preparation process, and the method is safe to use.

[0022] (3) The technical method of the present invention is simple, practical, mild in reaction conditions, easy in construction and operation, high in productivity, high in repeatability, and has no excessively high requirements on equipment. It can be used for large-scale experiments and has significant economic, environmental and social effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the Si-ZVI prepared in Example 1 wet ([Si / Fe]=0.01) and SEM-mapping images of ZVI prepared in Comparative Example 1.

[0024] Figure 2 Si-ZVI prepared in Example 1 wet ([Si / Fe]=0.01) and TEM images of ZVI prepared in Comparative Example 1.

[0025] Figure 3 The comparison chart of TCE removal effect in Application Example 1; wherein: ZVI is the zero-valent iron material prepared in Comparative Example 1, ZVI wet The wet-ground zero-valent iron material obtained in Comparative Example 2, Si-ZVI dry (Si / Fe=0.01) represents the dry-ground sodium silicate doped zero-valent iron material obtained in Comparative Example 3, Si-ZVI wet (Si / Fe=0.01) represents the wet-ground sodium silicate doped zero-valent iron material obtained in Example 1, Si-ZVI wet (Si / Fe=0.05) represents the wet-ground sodium silicate doped zero-valent iron material prepared in Example 2.

[0026] Figure 4 The comparison chart of the removal effect of Trans-1,2-DCE in Application Example 2; wherein: ZVI is the zero-valent iron material prepared in Comparative Example 1, Si-ZVI wet It represents the wet-ground silicon-doped zero-valent iron material prepared in Example 1.

[0027] Figure 5 The comparison chart of CF removal effect in Application Example 3; wherein: ZVI is the zero-valent iron material prepared in Comparative Example 1, Si-ZVI wetIt represents the wet-ground silicon-doped zero-valent iron material prepared in Example 1.

[0028] Figure 6 The comparison chart of the removal effect of 1,1-DCE in Application Example 4; wherein: ZVI is the zero-valent iron material prepared in Comparative Example 1, Si-ZVI wet It represents the wet-ground silicon-doped zero-valent iron material prepared in Example 1. DETAILED DESCRIPTION

[0029] In order to make those skilled in the art better understand the scheme of the present invention, the technical scheme of the present invention is clearly and completely described below in conjunction with specific embodiments. It should be noted that the following detailed descriptions are all exemplary and are only embodiments of a part of the present invention, rather than all embodiments.

[0030] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative work should fall within the scope of protection of the present invention.

[0031] Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those of ordinary skill in the art to which this application belongs. The experimental materials used in the examples of the present invention are all conventional experimental materials in the art and can be purchased through commercial channels. Experimental methods without specifying detailed conditions were performed according to conventional experimental methods or according to the operating instructions recommended by the supplier.

[0032] The main raw materials involved in the following implementation, such as reduced iron powder (cZVI) from Aladdin (Shanghai, China), silicic acid from Aladdin (Shanghai, China), all reagents are analytically pure, wherein the reduced iron powder particle size is 28 μm, and the silicic acid is in powder form. The ball milling medium used is a zirconia ball milling bead with a particle size of 6 mm, the ball milling speed is adjusted to 300-500 rpm, and the ball milling time is 2-30 h. After the ball milling is completed, the obtained iron-based material is separated from the grinding medium with a sieve under a nitrogen atmosphere.

[0033] In the following specific embodiments, oxygen-free water is prepared by purging deionized water with N2 for one hour and storing it in a glove box filled with Ar, ZVI is a zero-valent iron material, and Si-ZVI wet is a silicon-doped zero-valent iron composite material, and [Si / Fe] represents the molar ratio of silicate to zero-valent iron.

[0034] Example 1

[0035] 2.4656g of reduced iron powder and 0.0343g of silicic acid were placed in a ball mill, 69μL of oxygen-free water was added, and the jar was filled with argon; after being placed in a planetary ball mill for 20h, a silicon-doped zero-valent iron composite material Si-ZVI with a ratio of silicic acid to zero-valent iron substance of 0.01:1 was obtained.wet ([Si / Fe]=0.01).

[0036] The ball milling medium used was zirconia ball milling beads with a particle size of 6 mm, the ball milling speed was adjusted to 400 rpm, and the ball milling time was 20 h. After the ball milling was completed, the wet-milled silicon-doped zero-valent iron composite material (Si-ZVI) was screened under a nitrogen atmosphere. wet ) were separated from the grinding media and the material was stored in glass bottles under anaerobic environment.

[0037] Si-ZVI prepared in Example 1 wet The TEM image is as follows Figure 1 As shown, the successful doping of Si element and the uniform distribution of each element can be clearly seen.

[0038] Example 2

[0039] 2.3372g of reduced iron powder and 0.1627g of silicic acid were placed in a ball mill, 69μL of oxygen-free water was added, and the jar was filled with argon gas; after being placed in a planetary ball mill for 10h, a silicon-doped zero-valent iron composite material Si-ZVI with a ratio of silicic acid to zero-valent iron substance of 0.05:1 was obtained. wet ([Si / Fe]=0.05).

[0040] The ball milling medium used was zirconia ball milling beads with a particle size of 6 mm, the ball milling speed was adjusted to 400 rpm, and the ball milling time was 10 h. After the ball milling was completed, the wet-milled silicon-doped zero-valent iron composite material (Si-ZVI) was screened under a nitrogen atmosphere. wet ) were separated from the grinding media and the material was stored in glass bottles under anaerobic environment.

[0041] Example 3

[0042] 2.3431 g of reduced iron powder and 0.1569 g of silicic acid were placed in a ball mill, 69 μL of oxygen-free water was added, and the jar was filled with argon gas; after being placed in a planetary ball mill for 2 hours, a silicon-doped zero-valent iron composite material Si-ZVI with a ratio of silicic acid to zero-valent iron substance of 0.03:1 was obtained. wet ([Si / Fe]=0.03).

[0043] The ball milling medium used was zirconia ball milling beads with a particle size of 6 mm, the ball milling speed was adjusted to 400 rpm, and the ball milling time was 2 h. After the ball milling was completed, the wet-milled silicon-doped zero-valent iron composite material (Si-ZVI) was screened under a nitrogen atmosphere. wet ) were separated from the grinding media and the material was stored in glass bottles under anaerobic environment.

[0044] Comparative Example 1

[0045] 2.5 g of reduced iron powder was placed in a ball milling jar, and the jar was filled with argon; after being placed in a planetary ball mill and ball milled for 20 hours, ZVI was obtained. The ball milling medium used was zirconia ball milling beads with a particle size of 6 mm, the ball milling speed was adjusted to 400 rpm, and the ball milling time was 20 hours. After the ball milling was completed, the obtained ball milled zero-valent iron (ZVI) was separated from the grinding medium with a sieve under a nitrogen atmosphere, and the material was stored in a glass bottle under an anaerobic environment.

[0046] Si-ZVI prepared in Example 1 wet The SEM image of ZVI obtained in Comparative Example 1 is as follows: Figure 2 As shown, from Figure 1 It can be seen that the surface morphology of ZVI is regular and the particles are relatively large. wet The particle size of the material is small, the particle surface has many wrinkles, and the specific surface area is increased. This shows that under the action of mechanical force, the incorporation of Si causes a significant change in the particle size and specific surface area of ​​ZVI. Figure 1 It can be seen that Si-ZVI L The Fe, O and Si elements of the material are evenly distributed on the surface of the particles. Figure 2 The successful doping of Si element and the uniform distribution of various elements can also be clearly seen in the TEM image.

[0047] Comparative Example 2

[0048] Take 2.5g of reduced iron powder and place it in a ball mill, add 69μL of oxygen-free water, and fill the jar with argon; place it in a planetary ball mill and mill it for 2h to obtain wet-milled zero-valent iron material ZVI. wet .

[0049] The ball milling medium used was zirconia ball milling beads with a particle size of 6 mm, the ball milling speed was adjusted to 400 rpm, and the ball milling time was 2 h. After the ball milling was completed, the obtained wet-ground zero-valent iron material (ZVI) was screened under a nitrogen atmosphere. wet ) were separated from the grinding media and the material was stored in glass bottles under anaerobic environment.

[0050] Comparative Example 3

[0051] Weigh 2.4656g of reduced iron powder and 0.0343g of silicic acid and place them in a ball milling jar, which is then filled with argon gas. After being placed in a planetary ball mill and ball milled for 20h, dry-milled silicon-doped zero-valent iron material Si-ZVI is obtained. dry ([Si / Fe]=0.01).

[0052] The ball milling medium used was zirconia ball milling beads with a particle size of 6 mm, the ball milling speed was adjusted to 400 rpm, and the ball milling time was 2 h. After the ball milling was completed, the obtained dry-ground silicon-doped zero-valent iron material (Si-ZVI) was screened under a nitrogen atmosphere. dry) were separated from the grinding media and the material was stored in glass bottles under anaerobic environment.

[0053] Application Example 1

[0054] 26 mL of buffer solution (4-hydroxyethylpiperazineethanesulfonic acid) was added to each of 5 groups of 52 mL serum bottles, and 0.26 g of ZVI prepared in Comparative Example 1 and 0.26 g of ZVI prepared in Comparative Example 2 were added respectively. wet , 0.26 g Si-ZVI prepared in Comparative Example 3 dry , 0.26 g Si-ZVI prepared in Example 1 wet , 0.26 g Si-ZVI prepared in Example 2 wet , add 19 microliters of 17.9g / L TCE solution to make its initial concentration 100 micromolar. Finally, send the serum bottle into a 25°C constant temperature incubator and place it on a rotating incubator with a speed of n=30rpm for continuous and thorough mixing reaction.

[0055] At the designed sampling time point, 100 μL of the headspace gas from the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the TCE concentration in the serum bottle at the sampling time point. The experimental results are as follows: Figure 3 As shown. Through linear fitting, it can be obtained that the degradation rate of wet-milled silicon-doped zero-valent iron composite material with [Si / Fe] = 0.01 is 34 times that of zero-valent iron material. wet The degradation rate of Si-ZVI with [Si / Fe] of 0.05 is wet 19.7 times of that.

[0056] Application Example 2

[0057] 26 mL of buffer solution was added to each of the two 52 mL serum bottles, and 0.26 g of ZVI prepared in Comparative Example 1 and Si-ZVI prepared in Example 1 were added respectively. wet , add 20 microliters of 12.659 g / L trans-1,2-DCE solution to each, so that the initial concentration is 100 micromolar. Finally, send the serum bottle to a 25°C constant temperature incubator and place it on a rotating incubator with a speed of n=30 rpm for uninterrupted and thorough mixing reaction.

[0058] At the designed sampling time point, 100 μL of the headspace gas from the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the trans-DCE concentration in the serum bottle at the sampling time point. The experimental results are shown in the figure. Figure 4 As shown in Figure 2, the degradation rate of Si-ZVIwet is 25.6 times that of ZVI through linear fitting. This indicates that the composite material modified by ball milling can greatly improve the removal effect of trans-1,2-DCE.

[0059] Application Example 3

[0060] 26 mL of buffer solution was added to each of the two 52 mL serum bottles, and 0.26 g of ZVI prepared in Comparative Example 1 and Si-ZVI prepared in Example 1 were added respectively. wet , 21 μl of 14.8 g / L CF solution was added to each, making the initial concentration 100 μmol. Finally, the serum bottle was sent to a 25°C constant temperature incubator and placed on a rotating incubator with a speed of n=30 rpm for continuous and thorough mixing reaction.

[0061] At the designed sampling time node, 100 μL of the headspace gas in the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the CF concentration in the serum bottle at the sampling time node. The experimental results are as follows: Figure 5 As shown. Through linear fitting, it can be obtained that Si-ZVI with [Si / Fe] of 0.01 wet The degradation rate of ZVI is 5.8 times that of ZVI, which indicates that the composite material modified by ball milling can greatly improve the removal effect of CF.

[0062] Application Example 4

[0063] 26 mL of buffer solution was added to each of the two 52 mL serum bottles, and 0.26 g of ZVI prepared in Comparative Example 1 and Si-ZVI prepared in Example 1 were added respectively. wet , 21 microliters of 12.23 g / L 1,1-DCE solution was added to each, making the initial concentration 100 micromolar. Finally, the serum bottle was sent to a 25°C constant temperature incubator and placed on a rotating incubator with a speed of n=30 rpm for continuous and thorough mixing reaction.

[0064] At the designed sampling time point, 100 μL of the headspace gas from the serum bottle was extracted with a sampling needle and injected into the GC-FID to measure the 1,1-DCE concentration in the serum bottle at the sampling time point. The experimental results are as follows: Figure 6 As shown. Through linear fitting, it can be obtained that Si-ZVI with [Si / Fe] of 0.01 wet The degradation rate of ZVI is 10.3 times that of ZVI. This indicates that the composite material modified by ball milling can greatly improve the removal effect of 1,1-DCE.

Claims

1. A method for preparing a wet-milled silicon-doped zero-valent iron composite material, characterized in that: Silicic acid powder and zero-valent iron powder are mixed, oxygen-free water is added, and ball milling is performed in an inert gas atmosphere or a vacuum environment to obtain a wet-milled silicon-doped zero-valent iron composite material.

2. The method for preparing the wet-milled silicon-doped zero-valent iron composite material according to claim 1, characterized in that: The molar ratio of the iron to silicate is 1:0.01-0.

05.

3. The method for preparing the wet-milled silicon-doped zero-valent iron composite material according to claim 1, characterized in that: The mass volume ratio of the zero-valent iron powder to oxygen-free water is 1 g:25-30 μL.

4. The method for preparing the wet-milled silicon-doped zero-valent iron composite material according to claim 1, characterized in that: The mass volume ratio of the silicic acid, zero-valent iron powder mixture to oxygen-free water is 0.030-0.040 g / μL.

5. The method for preparing the wet-milled silicon-doped zero-valent iron composite material according to claim 1, characterized in that: The zero-valent iron powder is elemental iron powder, original iron powder, cast iron powder, pig iron powder or industrial waste iron filings containing zero-valent iron, and the particle size of the reduced iron powder material is 2 to 30 μm.

6. The method for preparing the wet-milled silicon-doped zero-valent iron composite material according to claim 1, characterized in that: The ball milling operation is as follows: a planetary ball mill is used for ball milling, the ball milling speed is 300 to 500 rpm, and the ball milling time is 2 to 30 hours.

7. The method for preparing the wet-milled silicon-doped zero-valent iron composite material according to claim 1, characterized in that: Sodium silicate powder and iron powder are mixed in proportion and then placed in a ball milling jar of a planetary ball mill for ball milling. The ball milling jar is filled with zirconium oxide beads as a ball milling medium, and the filling amount of the ball milling medium is 8-20% of the volume of the ball milling jar cavity.

8. A wet-ground silicon-doped zero-valent iron composite material obtained by the preparation method according to any one of claims 1 to 7.

9. Use of the wet-ground silicon-doped zero-valent iron composite material obtained by the preparation method of any one of claims 1 to 7 or the wet-ground silicon-doped zero-valent iron composite material according to claim 8 in the repair of water bodies polluted by chlorine-containing organic pollutants and heavy metals.

10. The use according to claim 9, characterized in that: The chlorine-containing organic pollutant is at least one of chloroform, trichloroethylene, 1,1-dichloroethylene and trans-1,2-dichloroethylene.

Citation Information

Patent Citations

  • Silicification modified zero-valent iron and preparation method and application thereof

    CN112250156A

  • Sodium silicate modified zero-valent iron composite material as well as preparation method and application thereof

    CN114735799A