Infrared-temperature composite sensing chalcogenide glass optical fiber as well as preparation method and application thereof
Through infrared-temperature composite sensing chalcogenide glass optical fiber, using its Seebeck effect and infrared evanescent wave effect, it solves the problem of difficulty in monitoring human body surface temperature and biomarkers simultaneously with existing equipment, and achieves efficient and accurate health monitoring. monitoring, and has good mechanical flexibility and simple preparation method.
Patent Information
- Application Number
- CN202410728201.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing wearable health monitoring devices to simultaneously monitor human body surface temperature and biomarkers, and the sensors have insufficient rigidity and breathability, resulting in inaccurate data recording and difficulty in long-term use.
Develop an infrared-temperature composite sensing chalcogenide glass optical fiber. Through the excellent Seebeck effect and infrared evanescent wave effect, it can simultaneously monitor the human body surface temperature and the type and concentration of biomarkers. It uses the chemistry of chalcogenide glass materials. The composition is AsxSe1-x-yTey, Ge0.1As0.9-m-nSemTen and GepSe1-p-qTeq. It is prepared as a structural optical fiber and composited with fabric for use in human body wearable health monitoring equipment.
It achieves simultaneous monitoring of human body surface temperature and biomarkers, has no crosstalk between signals, has a simple preparation method, has excellent mechanical flexibility, is suitable for human body wearable health monitoring equipment, and improves the accuracy and reliability of monitoring.
Smart Images

Figure CN118724469A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical fiber sensing, and in particular relates to an infrared-temperature composite sensing chalcogenide glass optical fiber and a preparation method and application thereof. Background Art
[0002] Early screening and early detection of chronic and acute diseases can promote the transformation of disease treatment to health management and promote health throughout the life cycle. Developing real-time personal health monitoring technology is one of the keys. Wearable sensors can measure abnormalities in physical quantities or chemical components in real time and promptly reflect information about human health status. They have the advantages of high efficiency, low cost, low power consumption and convenience, and are of great significance to human health management and disease diagnosis.
[0003] However, most wearable devices on the market are currently limited to physical monitoring of the body surface, such as body temperature, heart rate, etc., and it is difficult to touch the real metabolites of the human body. Moreover, in terms of human health management, the monitoring of a single physiological signal is difficult to capture pathological information, and it is necessary to collect multiple physiological signals for comprehensive analysis. For example, patients with hyperthyroidism will cause a simultaneous increase in body temperature and lactic acid concentration in sweat, while patients with acute heart failure will cause a simultaneous decrease in body temperature and urea concentration in sweat. Monitoring of only a single physiological information such as body temperature, heart rate, and concentration of surface metabolites is of limited use in the screening and diagnosis of chronic and acute diseases. Therefore, the realization of real-time detection of human body temperature measurement and surface metabolite concentration is of great significance for disease diagnosis and treatment.
[0004] Both body temperature and sweat information can be obtained through surface monitoring technology. Combining the two can provide more comprehensive and accurate information for disease diagnosis and prevention. Traditional health monitoring methods usually rely on large equipment and professional medical personnel, which makes monitoring inconvenient and costly. Wearable monitoring systems can record users' body information in real time and assess their health level, which is of great significance in medical treatment, disease prevention and control. At present, the internal sensors of commercial wearable health monitoring devices such as smart watches are made of rigid semiconductor materials. When the body performs large movements, the rigid sensors are prone to detachment, resulting in inaccurate data recording and inability to monitor biomarkers. Although the developing electrochemical flexible sensor devices can realize body temperature and biomarker sensing, they still have the shackles of poor air permeability, complex operation, and difficulty in long-term reuse. Therefore, the research and development of new flexible sensing materials and devices is of great significance for the construction of wearable health monitoring systems.
[0005] Sulfur-based glass fibers have been widely studied in the fields of temperature sensing and infrared sensing in recent years due to their natural flexibility and unique Seebeck effect and infrared evanescent wave effect. Based on the Seebeck effect, temperature changes can be converted into corresponding voltage changes to achieve temperature detection; based on the infrared evanescent wave effect, qualitative and quantitative detection of biomarker types and concentrations can be achieved through characteristic infrared absorption spectra. However, to date, only single infrared or temperature sensing has been achieved in chalcogenide glass fibers, and chalcogenide glass fibers for simultaneous infrared and temperature monitoring have not been reported. This is mainly due to the mutual restriction between the infrared transmittance and thermoelectric properties of chalcogenide glass. Chalcogenide glass fibers with high Seebeck coefficients have relatively narrow transmission windows, while chalcogenide glass fibers with wide infrared transmittance usually need to contain Te elements with large atomic weight, have poor thermal stability, and are prone to crystallization during the fiber drawing process, resulting in degradation of their optical and electrical properties. Therefore, the development of chalcogenide glass fibers with both high Seebeck coefficients and wide infrared transmittance ranges is crucial for the real-time monitoring of body surface metabolites and body temperature. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention proposes an infrared-temperature composite sensing chalcogenide glass optical fiber and its preparation method and application. The chalcogenide glass optical fiber has excellent Seebeck effect and infrared evanescent wave effect, and can be used as a sensing medium in wearable health monitoring equipment for the human body, providing a new solution for the simultaneous monitoring of human body surface temperature and the types and concentrations of biomarkers.
[0007] The technical solution adopted by the present invention to solve the above technical problems is: infrared-temperature composite sensing chalcogenide glass optical fiber, the chalcogenide glass optical fiber is made of chalcogenide glass material, the chemical composition formula of the chalcogenide glass material is As x Se 1-x- y Te y ,Ge 0.1 As 0.9-m-n Se m Te n and Ge p Se 1-p-q Te q One of the following, wherein 0.2≤x≤0.3, 0.1≤y≤0.3, 0≤m≤0.4, 0.2≤n≤0.7, 0.1≤p≤0.4, 0.2≤q≤0.5, and x, y, m, n, p and q are mole fractions respectively.
[0008] Preferably, the chalcogenide glass optical fiber is a structured optical fiber, and the structured optical fiber is a chalcogenide glass tapered optical fiber, a chalcogenide glass flat optical fiber or a chalcogenide glass ring optical fiber.
[0009] In a specific embodiment, the chalcogenide glass optical fiber is a chalcogenide glass tapered optical fiber, the tapered waist diameter of which is 10-100 μm and the tapered waist length of which is 10-30 mm.
[0010] The method for preparing the infrared-temperature composite sensing chalcogenide glass optical fiber comprises the following steps:
[0011] Step 1, preparing a matrix chalcogenide glass round rod: preparing a glass round rod by a melt quenching method according to the chemical composition of the chalcogenide glass material, and annealing the glass round rod immediately after it is formed to obtain a matrix chalcogenide glass round rod;
[0012] Step 2, preparing an optical fiber preform: polishing and cleaning the surface of the matrix chalcogenide glass round rod to obtain an optical fiber preform;
[0013] Step 3, drawing chalcogenide glass optical fiber: vertically placing the optical fiber preform in the furnace of the drawing tower, then continuously introducing inert gas into the furnace, heating the furnace, and when the temperature inside the furnace approaches the glass softening temperature of the chalcogenide glass material, starting to draw the optical fiber, continuously introducing inert gas into the furnace during the drawing process, and regulating the lowering speed and drawing speed of the optical fiber preform, and finally obtaining the chalcogenide glass optical fiber;
[0014] Step 4, preparing a structured optical fiber: preparing the chalcogenide glass optical fiber into the structured optical fiber.
[0015] Preferably, the structured optical fiber is a chalcogenide glass tapered optical fiber. In step 4, the chalcogenide glass tapered optical fiber is obtained by a melt-tapering method, and the process is: a fiber clamp is fixed on a displacement platform, two ends of the chalcogenide glass optical fiber are respectively fixed on the fiber clamp, a heating source is used to uniformly heat the middle part of the chalcogenide glass optical fiber for 10-20s, and then the displacement platform is moved to uniformly taper to obtain the chalcogenide glass tapered optical fiber.
[0016] Preferably, the structured optical fiber is a chalcogenide glass flat-plate optical fiber. In step 4, a flat heating method is used to obtain a chalcogenide glass flat-plate optical fiber, and the process is as follows: 1) fixing the two ends of the chalcogenide glass optical fiber on the optical fiber clamps respectively, and fixing and straightening the optical fiber by using the optical fiber clamps, so that the middle part of the chalcogenide glass optical fiber is parallel to the planes of the two hot pressing molds, and then clamping the middle part of the chalcogenide glass optical fiber by the two hot pressing molds; 2) increasing the temperature of the hot pressing mold, heating the middle part of the chalcogenide glass optical fiber by the hot pressing mold, and keeping the temperature for 20-30 seconds after the temperature of the hot pressing mold reaches the glass softening temperature of the chalcogenide glass material; 3) fixing a clamping device above the hot pressing mold and pressurizing the hot pressing mold by an elastic clamp, so that the middle part of the chalcogenide glass optical fiber is compressed and deformed; 4) keeping the pressure constant and gradually reducing the temperature of the hot pressing mold; 5) after the temperature of the hot pressing mold cools to room temperature, removing the chalcogenide glass optical fiber, and cleaning the surface of the middle part of the chalcogenide glass optical fiber with deionized water and alcohol to obtain a chalcogenide glass flat-plate optical fiber.
[0017] Preferably, the structured optical fiber is a chalcogenide glass ring optical fiber. In step 4, a heating bending method is used to obtain the chalcogenide glass ring optical fiber, and the process is as follows: the chalcogenide glass optical fiber is placed on a disc with a scale, and the disc is fixed on a bracket, and then a ceramic heating rod fixed by a clamp is vertically placed in the middle of the disc, and then the ceramic heating rod is heated to the glass softening temperature of the chalcogenide glass material, and then the chalcogenide glass optical fiber is slowly bent around the ceramic heating rod; after the number of bending turns of the chalcogenide glass optical fiber reaches a predetermined number of turns, the clamp is moved upward, and the bent chalcogenide glass optical fiber is removed from the ceramic heating rod, so as to obtain a chalcogenide glass ring optical fiber with a predetermined bending radius and number of bending turns.
[0018] The infrared-temperature composite sensing chalcogenide glass optical fiber of the present invention can be used as a sensing medium in wearable health monitoring equipment for the human body, converting the biochemical information and physical information of the human body surface into optical signals and electrical signals respectively, thereby realizing simultaneous monitoring of the human body surface temperature and the types and concentrations of biomarkers.
[0019] The infrared-temperature composite sensing chalcogenide glass optical fiber of the present invention is used as a sensing medium, and the working principle of infrared sensing is: for infrared sensing, when light propagates inside the chalcogenide glass optical fiber, the evanescent wave generated on the surface of the optical fiber can capture the excitation of the vibration mode of the chemical bond in the molecule in contact with it. The fingerprint region of most chemical and biological molecules, that is, the characteristic absorption region formed by the vibration rotation energy level transition of the chemical bond, is located in the mid-infrared region (2.5-25μm). When the optical fiber contacts the sample to be tested (such as human sweat), the evanescent wave of a specific frequency is absorbed by the chemical bond vibration contained in the test object and causes an infrared characteristic absorption peak to appear on the output spectrum. By analyzing the peak shape of the infrared absorption spectrum and the changes in the absorption peak intensity, accurate monitoring of specific solutions and changes in solution concentration can be achieved. In addition, by increasing the total number of reflections N of light at the optical fiber / sample interface, the selective absorption of the evanescent wave at a specific wavelength by the sample can be promoted, which can be expressed by the following formula:
[0020]
[0021] Among them, L, d and θ i Respectively represent the fiber length, fiber diameter and light incident angle of the sensing area. Obviously, N is inversely proportional to the fiber diameter, that is, reducing the fiber diameter of the sensing area can improve the sensitivity of the test.
[0022] The infrared-temperature composite sensing chalcogenide glass optical fiber of the present invention is used as a sensing medium, and the working principle of temperature sensing is: for temperature sensing, the chalcogenide glass optical fiber has an excellent Seebeck effect. When the temperature at both ends of the optical fiber changes, the carriers will accumulate at the hot end, thereby generating a voltage difference at both ends of the optical fiber. Therefore, by integrating the infrared evanescent wave effect and the Seebeck effect of the chalcogenide glass optical fiber, the biochemical information and physical information of the human body surface can be converted into optical signals and electrical signals respectively, realizing the simultaneous monitoring of the human body surface temperature and the types and concentrations of biomarkers.
[0023] The infrared-temperature composite sensing chalcogenide glass optical fiber of the present invention has excellent mechanical flexibility, can be composited with fabric, and is applied to wearable health monitoring equipment for the human body.
[0024] When the infrared-temperature composite sensing chalcogenide glass optical fiber of the present invention is used as a sensing medium in a wearable health monitoring device for a human body, the monitored biomarkers include but are not limited to at least one of lactic acid, urea, glucose and alcohol in sweat.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] (1) The infrared-temperature composite sensing chalcogenide glass optical fiber of the present invention has both excellent Seebeck effect and infrared evanescent wave effect, and can be used as a sensing medium in wearable health monitoring equipment for the human body, converting the biochemical information and physical information of the human body surface into optical signals and electrical signals respectively, thereby realizing simultaneous monitoring of the human body surface temperature and the types and concentrations of biomarkers;
[0027] (2) The infrared-temperature composite sensing chalcogenide glass optical fiber of the present invention can convert the biochemical information and physical information of the human body surface into optical signals and electrical signals respectively, without crosstalk between the signals and without the need for additional calibration compensation;
[0028] (3) The infrared-temperature composite sensing sulfur-based glass optical fiber of the present invention has a simple preparation method, has excellent mechanical flexibility, can be composited with fabrics, and is applied to wearable health monitoring equipment for the human body. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a structural schematic diagram of the detection system built in the embodiment;
[0030] Figure 2 is a graph showing the relationship between the absorption intensity of the chalcogenide glass tapered optical fiber prepared in Example 1 at 8.85 μm and 9.54 μm in a lactic acid solution and different lactic acid volume concentrations;
[0031] Figure 3 is an infrared spectrum of the chalcogenide glass tapered optical fiber prepared in Example 1 when the volume concentration of lactic acid is 24%;
[0032] Figure 4 is a curve showing the output voltage of the chalcogenide glass tapered optical fiber prepared in Example 1 changing with temperature;
[0033] Figure 5 is a graph showing the relationship between the absorption intensity of the chalcogenide glass flat optical fiber prepared in Example 2 at 6.82 μm in a urea solution and different urea volume concentrations;
[0034] Figure 6 is an infrared spectrum of the chalcogenide glass flat optical fiber prepared in Example 2 when the urea volume concentration is 20%;
[0035] Figure 7 is a graph showing the relationship between the absorption intensity of the chalcogenide glass ring optical fiber prepared in Example 3 at 9.25 μm and 9.65 μm in a glucose solution and different glucose volume concentrations;
[0036] Figure 8 This is the infrared spectrum of the chalcogenide glass ring optical fiber prepared in Example 3 when the volume concentration of glucose is 20%. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with the embodiments of the drawings. The equipment, devices or structures not limited by the present invention all adopt conventional technical means in the art.
[0038] The infrared-temperature composite sensing chalcogenide glass optical fiber of Example 1 is composed of a chemical composition formula of Ge 0.1 As 0.3 Se 0.4 Te 0.2 The chalcogenide glass material is composed of the following steps:
[0039] Step 1, preparing a matrix chalcogenide glass round rod: using 5N purity Ge, As, Se, and Te as raw materials, and mixing them according to the chemical composition of the chalcogenide glass material, weighing and mixing the raw materials according to the required weight in a glove box filled with inert gas; placing the mixed raw materials into a pre-cleaned quartz tube with a pore size of 15 mm, and evacuating the quartz tube to 1.0×10 -3 After Pa, the quartz tube is sealed with a hydrogen-oxygen flame; the sealed quartz tube is placed in a rocking furnace, the temperature is slowly raised to 850°C, and the temperature is kept for melting for 12 hours while rocking. After the melting is completed, when the temperature drops to 700°C, the quartz tube containing the glass liquid is quickly placed in water for quenching, and then the quartz tube is quickly placed in an annealing furnace preheated to 180°C and kept for 4 hours for annealing. After the annealing is completed, when the temperature of the annealing furnace slowly drops to room temperature, the quartz tube is taken out and broken, thereby obtaining a matrix chalcogenide glass round rod;
[0040] Step 2, preparing an optical fiber preform: polishing the surface of the matrix chalcogenide glass round rod, and washing it with hydrochloric acid, anhydrous alcohol, and distilled water, respectively, to obtain an optical fiber preform with a diameter of 13 mm and a length of 70 mm;
[0041] Step 3, drawing chalcogenide glass optical fiber: vertically placing the optical fiber preform in the furnace of the drawing tower, and then continuously introducing inert gas into the furnace to heat the furnace. When the temperature inside the furnace is close to the glass softening temperature of the chalcogenide glass material, the optical fiber can be drawn. During the drawing process, inert gas is continuously introduced into the furnace, and the lowering speed and drawing speed of the optical fiber preform are regulated to finally obtain the chalcogenide glass optical fiber.
[0042] Step 4, prepare structured optical fiber: use the melt taper method to prepare the chalcogenide glass optical fiber into a chalcogenide glass tapered optical fiber, the process is: fix the optical fiber fixture on the displacement platform driven by the stepper motor, select the chalcogenide glass optical fiber with a length of 40cm and a diameter of 350μm, fix the two ends of the chalcogenide glass optical fiber on the optical fiber fixture respectively, use the heating source to uniformly heat the middle part of the chalcogenide glass optical fiber for 10-20s, and then uniformly taper the optical fiber by moving the displacement platform to obtain a double-tapered Ge with a waist diameter of 50μm and a waist length of 20mm. 0.1 As 0.3 Se 0.4 Te 0.2 Chalcogenide glass tapered optical fiber.
[0043] Build a detection system such as Figure 1 As shown in FIG. 1 , the detection system includes a Fourier transform infrared spectrometer 1, a zinc selenide focusing lens 2, a fiber fixture 3, a quartz liquid pool 5, a heating platform 6, a mercury cadmium telluride detector 8 and a computer 9, which are arranged in sequence. One end of the chalcogenide glass tapered optical fiber 4 is fixed to the fiber fixture 3, wherein the heating platform 6 is used to heat the chalcogenide glass tapered optical fiber 4. The detection system after construction is as shown in FIG. Figure 1 shown.
[0044] Detection process: The chalcogenide glass tapered optical fiber 4 (i.e., Ge 0.1 As 0.3 Se 0.4 Te 0.2 A chalcogenide glass tapered optical fiber) is placed in a quartz liquid pool 5, and artificial sweat with a lactic acid volume concentration of 0.8% is added to the quartz liquid pool 5. The temperature of the heating platform 6 is adjusted to 30.5-40.5°C to simulate the abnormal body temperature of a human body suffering from hyperthyroidism; then, the Fourier transform infrared spectrometer 1 is turned on, and the light source is input into the chalcogenide glass tapered optical fiber 4 through the zinc selenide focusing objective 2. When the light source passes through the tapered area of the chalcogenide glass tapered optical fiber 4, an evanescent wave is formed on the surface of the optical fiber, and a relationship curve between the absorption intensity of the optical fiber at 8.85μm and 9.54μm in the lactic acid solution and the lactic acid volume concentration of 0.8% is obtained. The above detection process is carried out for artificial sweat with lactic acid volume concentrations of 0.4%, 0.8%, 1.6%, 2.4%, and 3.2%, respectively, to obtain a relationship curve between the absorption intensity of the optical fiber at 8.85μm and 9.54μm in the lactic acid solution and different lactic acid volume concentrations, as shown in FIG. Figure 2 shown.
[0045] from Figure 2 It can be seen that as the optical fiber comes into contact with artificial sweat, the corresponding molecular groups of lactic acid vibrate to produce specific absorption peaks in the mid-infrared region of 8.85μm and 9.54μm. Figure 3As shown, when the volume concentration of lactic acid is 24%, the absorbance of the characteristic peak at 8.85 μm reaches 0.42, thereby achieving qualitative and quantitative analysis of the volume concentration of lactic acid in sweat.
[0046] Silver paste is applied to both ends of the chalcogenide glass tapered optical fiber 4 and connected to wires, which are then connected to a desktop multimeter 7 to detect the voltage change of the chalcogenide glass tapered optical fiber 4 under different temperature differences. Figure 4 As shown, when the temperature difference between the two ends of the chalcogenide glass tapered optical fiber 4 is increased from 5°C to 20°C, the Seebeck coefficient of the chalcogenide glass tapered optical fiber 4 is measured to be 1163 μV / K, indicating that the chalcogenide glass tapered optical fiber 4 has extremely high temperature sensitivity.
[0047] The infrared-temperature composite sensing chalcogenide glass optical fiber of Example 2 is composed of a chemical composition formula of As 0.3 Se 0.5 Te 0.2 The chalcogenide glass material is composed of the following steps:
[0048] Step 1, preparing a matrix chalcogenide glass round rod: using 5N purity As, Se, and Te as raw materials, according to the chemical composition of the chalcogenide glass material, weighing and mixing the raw materials according to the required weight in a glove box filled with inert gas; placing the mixed raw materials into a pre-cleaned quartz tube with a pore size of 20 mm, and evacuating the quartz tube to 1.0×10 -3 After Pa, the quartz tube is sealed with a hydrogen-oxygen flame; the sealed quartz tube is placed in a rocking furnace, the temperature is slowly raised to 850°C, and the temperature is kept for melting for 12 hours while rocking. After the melting is completed, when the temperature drops to 550°C, the quartz tube containing the glass liquid is quickly placed in water for quenching, and then the quartz tube is quickly placed in an annealing furnace preheated to 110°C and kept for 4 hours for annealing. After the annealing is completed, when the temperature of the annealing furnace slowly drops to room temperature, the quartz tube is taken out and broken, thereby obtaining a matrix chalcogenide glass round rod;
[0049] Step 2, preparing an optical fiber preform: polishing the surface of the matrix chalcogenide glass round rod, and washing it with hydrochloric acid, anhydrous alcohol, and distilled water, respectively, to obtain an optical fiber preform with a diameter of 18 mm and a length of 60 mm;
[0050] Step 3, drawing chalcogenide glass optical fiber: vertically placing the optical fiber preform in the furnace of the drawing tower, and then continuously introducing inert gas into the furnace to heat the furnace. When the temperature inside the furnace is close to the glass softening temperature of the chalcogenide glass material, the optical fiber can be drawn. During the drawing process, inert gas is continuously introduced into the furnace, and the lowering speed and drawing speed of the optical fiber preform are regulated to finally obtain the chalcogenide glass optical fiber.
[0051] Step 4, preparing a structured optical fiber: using a flat heating method to prepare a chalcogenide glass optical fiber into a chalcogenide glass flat optical fiber, the process is as follows: 1) fixing the two ends of the chalcogenide glass optical fiber on an optical fiber clamp respectively, and using the optical fiber clamp to fix and straighten the optical fiber so that the middle part of the chalcogenide glass optical fiber is parallel to the plane of the two hot pressing molds, and then clamping the middle part of the chalcogenide glass optical fiber up and down by the two hot pressing molds; 2) increasing the temperature of the hot pressing mold, heating the middle part of the chalcogenide glass optical fiber by the hot pressing mold, and keeping the temperature at 190° C. for 20-30 seconds after the temperature of the hot pressing mold reaches the glass softening temperature of the chalcogenide glass material; 3) fixing a clamping device above the hot pressing mold and pressurizing the hot pressing mold by an elastic clamp, so that the middle part of the chalcogenide glass optical fiber is compressed and deformed; 4) keeping the pressure constant and gradually reducing the temperature of the hot pressing mold; 5) after the temperature of the hot pressing mold cools to room temperature, removing the chalcogenide glass optical fiber, and cleaning the surface of the middle part of the chalcogenide glass optical fiber with deionized water and alcohol to obtain a chalcogenide glass flat optical fiber.
[0052] Using the detection system constructed in Example 1, the As in Example 2 0.3 Se 0.5 Te 0.2 The chalcogenide glass flat optical fiber is placed in a quartz liquid pool 5, and artificial sweat with a urea volume concentration of 0.5% is added to the quartz liquid pool 5. The temperature of the heating platform 6 is adjusted to 36.5-35.5°C to simulate the abnormal body temperature of a human body suffering from acute heart failure. Then, the Fourier transform infrared spectrometer 1 is turned on, and the light source is input to the As through the zinc selenide focusing lens 2. 0.3 Se 0.5 Te 0.2 In the chalcogenide glass flat fiber, when the light source passes through the flat area of the chalcogenide glass flat fiber, an evanescent wave will be formed on the surface of the fiber, and a curve of the relationship between the absorption intensity of the fiber at 6.82μm in the urea solution and the urea volume concentration of 0.5% is obtained. For artificial sweat with urea volume concentrations of 0.5%, 1%, 2%, 3%, and 4%, the above detection process is carried out respectively, and the curve of the relationship between the absorption intensity of the fiber at 6.82μm in the urea solution and different urea volume concentrations is obtained, as shown in FIG. Figure 5 As shown. Figure 5 It can be seen that as the optical fiber comes into contact with artificial sweat, the corresponding molecular group vibration of urea produces a specific absorption peak in the 6.82μm mid-infrared region. Figure 6 As shown, when the volume concentration of urea is 20%, the absorbance of the characteristic peak at 6.82 μm reaches 0.4, thereby achieving qualitative and quantitative analysis of the volume concentration of urea in sweat.
[0053] In As 0.3 Se 0.5 Te 0.2Silver paste was applied to both ends of the chalcogenide glass flat optical fiber and connected with wires, which were then connected to a desktop multimeter 7. When the temperature at one end of the optical fiber dropped from 36.5°C to 35.5°C, the voltage at both ends of the optical fiber dropped by 1.4 mV.
[0054] The infrared-temperature composite sensing chalcogenide glass optical fiber of Example 3 is composed of a chemical composition formula of Ge 0.2 Se 0.6 Te 0.2 The chalcogenide glass material is composed of the following steps:
[0055] Step 1, preparing a matrix chalcogenide glass round rod: using 5N purity Ge, Se, and Te as raw materials, and mixing them according to the chemical composition of the chalcogenide glass material, weighing and mixing the raw materials according to the required weight in a glove box filled with inert gas; placing the mixed raw materials into a pre-cleaned quartz tube with a pore size of 15 mm, and evacuating the quartz tube to 1.0×10 -3 After Pa, the quartz tube is sealed with a hydrogen-oxygen flame; the sealed quartz tube is placed in a rocking furnace, slowly heated to 900°C, and kept warm for 12 hours while rocking. After the melting is completed, when the temperature drops to 650°C, the quartz tube containing the glass liquid is quickly placed in water for quenching, and then the quartz tube is quickly placed in an annealing furnace preheated to 160°C and kept warm for 4 hours for annealing. After the annealing is completed, when the temperature of the annealing furnace slowly drops to room temperature, the quartz tube is taken out and broken, thereby obtaining a matrix chalcogenide glass round rod;
[0056] Step 2, preparing an optical fiber preform: polishing the surface of the matrix chalcogenide glass round rod, and washing it with hydrochloric acid, anhydrous alcohol, and distilled water, respectively, to obtain an optical fiber preform with a diameter of 13.5 mm and a length of 65 mm;
[0057] Step 3, drawing chalcogenide glass optical fiber: vertically placing the optical fiber preform in the furnace of the drawing tower, and then continuously introducing inert gas into the furnace to heat the furnace. When the temperature inside the furnace is close to the glass softening temperature of the chalcogenide glass material, the optical fiber can be drawn. During the drawing process, inert gas is continuously introduced into the furnace, and the lowering speed and drawing speed of the optical fiber preform are regulated to finally obtain the chalcogenide glass optical fiber.
[0058] Step 4, preparing a structured optical fiber: using a heating bending method to prepare a chalcogenide glass optical fiber into a chalcogenide glass ring optical fiber, the process is: placing the chalcogenide glass optical fiber on a disc with a scale, and fixing the disc on a bracket, and then vertically placing a ceramic heating rod fixed by a clamp in the middle of the disc, and then heating the ceramic heating rod to 250°C, and then slowly bending the chalcogenide glass optical fiber around the ceramic heating rod; after the number of bending turns of the chalcogenide glass optical fiber reaches a predetermined number of turns, the clamp is moved upward, and the bent chalcogenide glass optical fiber is removed from the ceramic heating rod, and a chalcogenide glass ring optical fiber with a predetermined bending radius and number of bending turns is obtained.
[0059] Using the detection system constructed in Example 1, the Ge 0.2 Se 0.6 Te 0.2 The chalcogenide glass ring optical fiber is placed in a quartz liquid pool 5, and artificial sweat with a glucose volume concentration of 0.5% is added to the quartz liquid pool 5. The temperature of the heating platform 6 is adjusted to 36.5-38.5°C to simulate the body temperature of a human body with diabetes and fever. Then, the Fourier transform infrared spectrometer 1 is turned on, and the light source is input into the Ge through the zinc selenide focusing lens 2. 0.2 Se 0.6 Te 0.2 In the chalcogenide glass ring fiber, when the light source passes through the ring area of the chalcogenide glass ring fiber, an evanescent wave will be formed on the surface of the fiber, and the absorption intensity of the fiber at 9.25μm and 9.65μm in the glucose solution and the glucose volume concentration of 0.5% are obtained. For artificial sweat with a glucose volume concentration of 0.5%, 1%, 2%, 3%, and 4%, the above detection process is carried out respectively, and the absorption intensity of the fiber at 9.25μm and 9.65μm in the glucose solution and the relationship curves of different glucose volume concentrations are obtained, as shown in FIG. Figure 7 As shown. Figure 7 It can be seen that as the optical fiber comes into contact with artificial sweat, the corresponding molecular groups of glucose vibrate to produce specific absorption peaks in the mid-infrared region of 9.25μm and 9.65μm. Figure 8 As shown, when the volume concentration of glucose is 20%, the absorbance of the characteristic peak at 9.25 μm reaches 0.35, thereby achieving qualitative and quantitative analysis of the volume concentration of glucose in sweat.
[0060] In Ge 0.2 Se 0.6 Te 0.2 Silver paste was applied to both ends of the chalcogenide glass ring optical fiber and connected with wires, which were then connected to a desktop multimeter 7. When the temperature at one end of the optical fiber increased from 36.5°C to 38.5°C, the voltage at both ends of the optical fiber increased by 2.45 mV.
Claims
1. Infrared-temperature composite sensing chalcogenide glass optical fiber, characterized in that: The chalcogenide glass optical fiber is made of chalcogenide glass material, and the chemical composition formula of the chalcogenide glass material is As x Se 1-x-y Te y ,Ge 0.1 As 0.9-m-n Se m Te n and Ge p Se 1-p-q Te q One of the following, wherein 0.2≤x≤0.3, 0.1≤y≤0.3, 0≤m≤0.4, 0.2≤n≤0.7, 0.1≤p≤0.4, 0.2≤q≤0.5, and x, y, m, n, p and q are mole fractions respectively.
2. The infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 1, characterized in that: The chalcogenide glass optical fiber is a structural optical fiber, and the structural optical fiber is a chalcogenide glass tapered optical fiber, a chalcogenide glass flat optical fiber or a chalcogenide glass ring optical fiber.
3. The infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 2, characterized in that: The chalcogenide glass optical fiber is a chalcogenide glass tapered optical fiber, the diameter of the tapered waist is 10-100 μm, and the length of the tapered waist is 10-30 mm.
4. The method for preparing the infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 2, characterized in that: The following steps are involved: Step 1, preparing a matrix chalcogenide glass round rod: preparing a glass round rod by a melt quenching method according to the chemical composition of the chalcogenide glass material, and annealing the glass round rod immediately after it is formed to obtain a matrix chalcogenide glass round rod; Step 2, preparing an optical fiber preform: polishing and cleaning the surface of the matrix chalcogenide glass round rod to obtain an optical fiber preform; Step 3, drawing chalcogenide glass optical fiber: vertically placing the optical fiber preform in the furnace of the drawing tower, then continuously introducing inert gas into the furnace, heating the furnace, and when the temperature inside the furnace approaches the glass softening temperature of the chalcogenide glass material, starting to draw the optical fiber, continuously introducing inert gas into the furnace during the drawing process, and regulating the lowering speed and drawing speed of the optical fiber preform, and finally obtaining the chalcogenide glass optical fiber; Step 4, preparing a structured optical fiber: preparing the chalcogenide glass optical fiber into the structured optical fiber.
5. The method for preparing the infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 4, characterized in that: The structured optical fiber is a chalcogenide glass tapered optical fiber. In step 4, a chalcogenide glass tapered optical fiber is obtained by a melt-tap method, and the process is as follows: a fiber clamp is fixed on a displacement platform, two ends of the chalcogenide glass optical fiber are respectively fixed on the fiber clamp, a heating source is used to uniformly heat the middle part of the chalcogenide glass optical fiber for 10-20 seconds, and then a uniform taper is performed by moving the displacement platform to obtain a chalcogenide glass tapered optical fiber.
6. The method for preparing the infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 4, characterized in that: The structural optical fiber is a chalcogenide glass flat-plate optical fiber. In step 4, a flat heating method is used to obtain a chalcogenide glass flat-plate optical fiber, and the process is as follows: 1) fixing the two ends of the chalcogenide glass optical fiber on the optical fiber clamps respectively, and using the optical fiber clamps to fix and straighten the optical fiber, so that the middle part of the chalcogenide glass optical fiber is parallel to the planes of the two hot pressing molds, and then the middle part of the chalcogenide glass optical fiber is clamped up and down by the two hot pressing molds; 2) increasing the temperature of the hot pressing mold, heating the middle part of the chalcogenide glass optical fiber through the hot pressing mold, and keeping the temperature for 20-30 seconds after the temperature of the hot pressing mold reaches the glass softening temperature of the chalcogenide glass material; 3) fixing a clamping device above the hot pressing mold and pressurizing the hot pressing mold through an elastic clamp, so that the middle part of the chalcogenide glass optical fiber is compressed and deformed; 4) keeping the pressure constant and gradually reducing the temperature of the hot pressing mold; 5) after the temperature of the hot pressing mold cools to room temperature, removing the chalcogenide glass optical fiber, and cleaning the surface of the middle part of the chalcogenide glass optical fiber with deionized water and alcohol to obtain a chalcogenide glass flat-plate optical fiber.
7. The method for preparing the infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 4, characterized in that: The structured optical fiber is a chalcogenide glass ring optical fiber. In step 4, a heating bending method is used to obtain the chalcogenide glass ring optical fiber, and the process is as follows: the chalcogenide glass optical fiber is placed on a disc with a scale, and the disc is fixed on a bracket, and then a ceramic heating rod fixed by a clamp is vertically placed in the middle of the disc, and then the ceramic heating rod is heated to the glass softening temperature of the chalcogenide glass material, and then the chalcogenide glass optical fiber is slowly bent around the ceramic heating rod; after the number of bending turns of the chalcogenide glass optical fiber reaches a predetermined number of turns, the clamp is moved upward, and the bent chalcogenide glass optical fiber is removed from the ceramic heating rod, so as to obtain a chalcogenide glass ring optical fiber with a predetermined bending radius and number of bending turns.
8. The use of the infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 1, characterized in that: This chalcogenide glass optical fiber is used as a sensing medium in wearable health monitoring equipment for the human body, converting the biochemical and physical information of the human body surface into optical signals and electrical signals respectively, thereby realizing simultaneous monitoring of the human body surface temperature and the types and concentrations of biomarkers.
9. The use of the infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 8, characterized in that: The chalcogenide glass optical fiber is composited with fabric and applied in wearable health monitoring equipment for human body.
10. The use of the infrared-temperature composite sensing chalcogenide glass optical fiber according to claim 8, characterized in that: The biomarker includes at least one of lactic acid, urea, glucose and alcohol in sweat.
Citation Information
Patent Citations
Preparation method and application of wafer with three-layer stacking structure
CN114864753A
Chalcogenide glass optical fiber monofilament and application of chalcogenide glass optical fiber monofilament in preparation of long-wave infrared optical fiber image transmission bundle
CN117310871A
Method for purifying starting materials for fabricating chalchogenide glass
US4801442A
Cited By
Chalcogenide glass optical fiber evanescent wave sensor integrating temperature sensing and preparation method thereof
CN122651637A
Temperature-aware chalcogenide glass optical fiber evanescent wave sensor and method of making same
CN122651637B